Materials / Compare

Aluminum 2024-T351 vs. Wood

Compare Aluminum 2024-T351 vs. Wood strength, stiffness, weight and thermal properties.

Change either side
Aluminum 2024-T351Wrought
WoodNatural
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Mechanical
Yield strength324MPasourcetypical, 0.2% offset, .500 in dia specimennot given (tensile used)
Ultimate tensile strength469MPasourcetypical99MPasourcemodulus of rupture (no direct tensile value)
Compressive strengthnot sourced46.6MPasourcecompression parallel to grain (maximum crushing strength), 12% MC
Flexural strengthnot sourced99MPasourcemodulus of rupture (static bending), 12% MC
Elongation at break19%sourcetypical, in 4Dnot sourced
Young's modulus (stiffness)73.1GPasourcetypical12.5GPasourcebending MOE, parallel to grain
Density2,770kg/m³sourcenominalnot sourced
Strength to weight117kN·m/kgnot sourced
Stiffness to weight26.4MN·m/kgnot sourced
Poisson's ratio0.33sourcetypical (handbook physical constant), all tempers0.35sourcemu_LR (red oak group, ~12% MC)
Shear modulus27.5GPa5.94x stiffer in shear4.63GPa
Bulk modulus71.7GPa13.9GPa
Speed of sound5,137m/snot sourced
Thermal
Thermal conductivity120W/m·Ksourcetypical, 20 °C0.18W/m·Ksourceacross grain, 12% MC (Table 4-7, approximate)
Thermal expansion22.9µm/m·Ksourcetypical, mean 20-100 °C3.1–4.5µm/m·Ksourceparallel to grain, ovendry wood, range across species
100 mm part over a 50 °C swing115µm growth19µm growth6.03x less
Specific heat875J/kg·Ksourcetypical, at 100 °C1,700J/kg·Ksourcesolid wood (all species), 12% MC, 27 C
Heats up and cools (diffusivity)49.5mm²/snot sourced
Thermal shock resistance15,561W/m63.8x more resistant244W/m
Melting point502–638°Csourcemelting rangenot sourced
Values for2024-T4/T351, Kaiser Aluminum sheet, coil & plate typical datasheet; Poisson from MIL-HDBK-5JNorthern red oak (Quercus rubra), clear straight-grained specimens at 12% MC, parallel to grain unless stated; USDA FPL Wood Handbook FPL-GTR-282 (2021) Ch. 4 and Ch. 5

Every value links to the document that states it. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Questions

Is Aluminum 2024-T351 stronger than Wood?

Aluminum 2024-T351 is stronger: its yield strength is 324 MPa against tensile strength 99 MPa for Wood (3.27x).

Which is stiffer, Aluminum 2024-T351 or Wood?

Aluminum 2024-T351 is stiffer: Young's modulus 73.1 GPa against 12.5 GPa for Wood, so the same part in Aluminum 2024-T351 deflects less under the same load.

Which conducts heat better, Aluminum 2024-T351 or Wood?

Aluminum 2024-T351 conducts heat better: 120 W/m·K against 0.18 W/m·K for Wood.

Which expands less with temperature?

Wood expands less: 3.8 µm/m·K against 22.9 µm/m·K for Aluminum 2024-T351.

Among 59 materials

1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonAluminumSteelIronTitaniumSteel AISI 1018Stainless 304Stainless 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless 303Stainless 17-4PHAluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelAluminum 2024-T351
Stiffness against density
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberAluminumSteelIronTitaniumSteel AISI 1018Stainless 304Stainless 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless 303Stainless 17-4PHAluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickAluminum 2024-T351
Strength against density

Related comparisons