Aluminum A380 (die-cast) strength, stiffness, density and thermal properties, with their source.
A bracket in Aluminum A380, as-cast finish.
| Process | Cast |
|---|
| Mechanical |
|---|
| Yield strength | 160MPasourcetypical, 25 °C |
|---|
| Ultimate tensile strength | 320MPasourcetypical, 25 °C |
|---|
| Elongation at break | 3.5%sourcetypical |
|---|
| Young's modulus (stiffness) | 71GPasourcetypical, 25 °C |
|---|
| Density | 2,713kg/m³sourcetypical at 68 °F |
|---|
| Strength to weight | 59kN·m/kg |
|---|
| Stiffness to weight | 26.2MN·m/kg |
|---|
| Poisson's ratio | not sourced |
|---|
| Shear modulus | not sourced |
|---|
| Bulk modulus | not sourced |
|---|
| Speed of sound | 5,116m/s |
|---|
| Thermal |
|---|
| Thermal conductivity | 96.2W/m·Ksourcetypical at 68 °F |
|---|
| Thermal expansion | 21.8µm/m·Ksourcetypical, 68-572 °F (20-300 °C) |
|---|
| 100 mm part over a 50 °C swing | 109µm growth |
|---|
| Specific heat | 963J/kg·Ksourcetypical at 68 °F |
|---|
| Heats up and cools (diffusivity) | 36.8mm²/s |
|---|
| Thermal shock resistance | not sourced |
|---|
| Values for | A380 aluminium high-pressure die-casting alloy, typical properties; Rheocast Company (aluminium die caster, Germantown WI) A380 alloy data page. |
|---|
Among 72 materials
Stiffness against densityStrength against density