Materials / Compare

Aluminum ADC12 vs. Brass C260

Compare Aluminum ADC12 vs. Brass C260 strength, stiffness, weight and thermal properties.

Aluminum ADC12Cast
Brass C260Wrought
MechanicalAluminum ADC12Brass C260
Yield strengthone test result149MPa1345MPa22.32x stronger
Ultimate tensile strengthone test result345MPa1427MPa224% stronger
Elongation at breakone test result2.3%123%210x more ductile
Young's modulus (stiffness)standard value79.8GPa3110GPa438% stiffer
Densitymeasured2,680kg/m³53.18x lighter8,525kg/m³4
Strength to weight55.6kN·m/kg37% higher40.5kN·m/kg
Stiffness to weight29.8MN·m/kg2.3x higher12.9MN·m/kg
Poisson's rationot sourced0.346
Shear modulusnot sourced41.2GPa
Bulk modulusnot sourced115GPa
Speed of sound5,457m/s1.52x faster3,597m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VNickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OMagnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum ADC12Brass C260
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VNickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OMagnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum ADC12Brass C260
Strength against densityHigher and further left: stronger for its weight
ThermalAluminum ADC12Brass C260
Thermal conductivity125W/m·K5121W/m·K4
Thermal expansionmeasured21µm/m·K520µm/m·K4
100 mm part over a 50 °C swing105µm growth100µm growth5% less
Specific heatmeasured911J/kg·K52.42x higher377J/kg·K4
Heats up and cools (diffusivity)51.2mm²/s36% faster37.7mm²/s
Thermal shock resistancenot sourced12,510W/m
Melting pointsolidus-liquidus515–582°C5solidus-liquidus916–954°C4
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VNickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OMagnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum ADC12Brass C260
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VNickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OMagnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum ADC12Brass C260
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources6 documents: Daiki Aluminium Industry, Copper Development Association, S.S. Aluminum, Wieland
Aluminum ADC12
JIS ADC12 (Al-Si-Cu, about A383 / EN AC-46100) high-pressure die-casting alloy, as cast; physical properties from Daiki Aluminium Industry (ADC12 ingot producer) measured values; modulus from S.S.Aluminum (ADC12 ingot producer) standard values.
Brass C260
C26000 cartridge brass, H02 half hard flat/strip: CDA Electronic Connector Design Guide (mechanical) + CDA alloy page (physical)
  1. 1
    NA Alloys Product DataDaiki Aluminium IndustryAluminum ADC12 · Yield strength: one test result, 0.2% proof stress, as cast, ASTM tensile bar (Daiki)Aluminum ADC12 · Ultimate tensile strength: one test result, as cast, ASTM tensile bar (Daiki)Aluminum ADC12 · Elongation at break: one test result, as cast, ASTM tensile bar (Daiki)
  2. 2
    Electronic Connector Design Guide: Cold Rolled TempersCopper Development Associationarchived copyBrass C260 · Yield strength: nominal, strip/flat, 0.5% extension (not 0.2% offset)Brass C260 · Ultimate tensile strength: nominal, strip/flatBrass C260 · Elongation at break: nominal, in 2.0 in., strip/flat
  3. 3
    Die-Casting Alloys (ダイカスト用合金)S.S. AluminumAluminum ADC12 · Young's modulus (stiffness): standard value (S.S.Aluminum)
  4. 4
    C26000 Alloy (copper.org)Copper Development Associationarchived copyBrass C260 · Young's modulus (stiffness): typical, temper-independentBrass C260 · Density: nominalBrass C260 · Thermal conductivity: typical, 20 °CBrass C260 · Thermal expansion: typical, mean 20-300 °CBrass C260 · Specific heat: typical, 20 °CBrass C260 · Melting point: solidus-liquidus
  5. 5
    DIK365 Product DataDaiki Aluminium IndustryAluminum ADC12 · Density: measured (Daiki)Aluminum ADC12 · Thermal conductivity: measured on specimens cut from a 50 x 100 x 5 mm flat die casting (Daiki)Aluminum ADC12 · Thermal expansion: measured, temperature range not stated (Daiki)Aluminum ADC12 · Specific heat: measured (Daiki)Aluminum ADC12 · Melting point: solidus-liquidus (Daiki)
  6. 6
    Wieland-M30 (CuZn30, C26000) Data SheetWielandarchived copyBrass C260 · Poisson's ratio: reference value at room temperature (Wieland-M30 = CuZn30 = C26000, rolled products)

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Questions

Mechanical

Is Aluminum ADC12 stronger than Brass C260?

Brass C260 is stronger: its yield strength is 345 MPa against 149 MPa for Aluminum ADC12 (2.32x).

Which is lighter, Aluminum ADC12 or Brass C260?

Aluminum ADC12 is lighter: 2,680 kg/m³ against 8,525 kg/m³ for Brass C260.

Which is stiffer, Aluminum ADC12 or Brass C260?

Brass C260 is stiffer: Young's modulus 110 GPa against 79.8 GPa for Aluminum ADC12, so the same part in Brass C260 deflects less under the same load.

Which is lighter for the same job, Aluminum ADC12 or Brass C260?

For the same stiffness or strength: Aluminum ADC12 is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.

Part that must beAluminum ADC12Brass C260
Stiff rod or tie (tension)lighter2.3x heavier
Stiff beam (bending)lighter2.71x heavier
Stiff panel or platelighter2.86x heavier
Strong rod or tielighter37% heavier
Strong beamlighter1.82x heavier
Strong panel or platelighter2.09x heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Aluminum ADC12 or Brass C260?

Brass C260 stretches further before it breaks: 23% elongation at break against 2.3% for Aluminum ADC12.

Thermal

Which conducts heat better, Aluminum ADC12 or Brass C260?

Aluminum ADC12 conducts heat better: 125 W/m·K against 121 W/m·K for Brass C260.

Which expands less with temperature?

Brass C260 expands less: 20 µm/m·K against 21 µm/m·K for Aluminum ADC12.

Related comparisons