Materials / Compare

Glass vs. Plastic Polycarbonate

Compare Glass vs. Plastic Polycarbonate strength, stiffness, weight and thermal properties.

GlassNatural
Plastic PolycarbonateBulk polymer (molded or machined)
MechanicalGlassPlastic Polycarbonate
Yield strengthnone (brittle)65MPa1
Ultimate tensile strength41MPa265MPa1
Flexural strengthmean MOR41MPa297MPa1
Elongation at breaknone (brittle)125%1
Young's modulus (stiffness)72GPa230x stiffer2.4GPa1
Density2,500kg/m³21,200kg/m³12.08x lighter
Strength to weight16.4kN·m/kg54.2kN·m/kg3.3x higher
Stiffness to weight28.8MN·m/kg14.4x higher2MN·m/kg
Poisson's ratio0.2220.383
Shear modulus29.5GPa33.9x stiffer in shear0.87GPa
Bulk modulus42.9GPa12.9x higher3.33GPa
Speed of sound5,367m/s3.79x faster1,414m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200Steel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30GlassPlastic Polycarbonate
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200Steel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30GlassPlastic Polycarbonate
Strength against densityHigher and further left: stronger for its weight
ThermalGlassPlastic Polycarbonate
Thermal conductivity0.937W/m·K24.68x more heat through a fin0.2W/m·K1
Thermal expansion8.3µm/m·K27.83x less65µm/m·K1
100 mm part over a 50 °C swing41.5µm growth7.83x less325µm growth
Specific heat880J/kg·K21,172J/kg·K433% higher
Heats up and cools (diffusivity)0.426mm²/s2.99x faster0.142mm²/s
Thermal shock resistance50.1W/m51.7W/m3% more resistant
Glass transitionnot sourced144°C1
Max service temperaturestrain point511°C2UL 746B RTI125°C1
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200Steel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30GlassPlastic Polycarbonate
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200Steel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30GlassPlastic Polycarbonate
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA sample part to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources4 documents: Covestro, Pilkington North America, Bayer MaterialScience
Glass
Annealed soda-lime-silica float glass, Pilkington North America Technical Bulletin ATS-129 (04/2025)
Plastic Polycarbonate
Covestro Makrolon 2405 general-purpose PC (MVR 19), Covestro technical datasheet version 2026-09-28, typical values
  1. 1
    Makrolon 2405 Technical Data SheetCovestroPlastic Polycarbonate · Yield strength: typical, tensile yieldPlastic Polycarbonate · Ultimate tensile strength: typical, stress at breakPlastic Polycarbonate · Flexural strength: typical, flexural strengthPlastic Polycarbonate · Elongation at break: typical, strain at breakPlastic Polycarbonate · Young's modulus (stiffness): typicalPlastic Polycarbonate · Density: typicalPlastic Polycarbonate · Thermal conductivity: typical, through-plane, 23 CPlastic Polycarbonate · Thermal expansion: typical, 23-55 C, parallel and normalPlastic Polycarbonate · Glass transition: typical, DSC 10 C/minPlastic Polycarbonate · Max service temperature: UL 746B RTI, tensile strength, 1.5 mm
  2. 2
    Technical Bulletin ATS-129: Properties of Soda-Lime Silica Float Glass (2025)Pilkington North Americaarchived copyGlass · Ultimate tensile strength: typical mean surface tensile stress at fracture (MOR), 60 s load, weathered, 50% breakage probabilityGlass · Flexural strength: mean MOR (same value as tensile)Glass · Young's modulus (stiffness): typicalGlass · Density: typicalGlass · Poisson's ratio: typicalGlass · Thermal conductivity: typical at 75 FGlass · Thermal expansion: typical, 75-575 FGlass · Specific heat: typical at 75 FGlass · Max service temperature: strain point (ASTM C336) - stress-relaxation onset, not a rated service limit
  3. 3
    Engineering Polymers Part and Mold Design: Thermoplastics, A Design GuideCovestroarchived copyPlastic Polycarbonate · Poisson's ratio: typical, polycarbonate family (Covestro Part and Mold Design guide, Table 3-1)
  4. 4
    Makrolon 2405 Data Sheet, ASTM valuesBayer MaterialSciencearchived copyPlastic Polycarbonate · Specific heat: typical (guide value), Bayer ASTM datasheet for Makrolon 2405, ASTM D 2766

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Questions

Mechanical

Is Glass stronger than Plastic Polycarbonate?

Plastic Polycarbonate is stronger: its yield strength is 65 MPa against tensile strength 41 MPa for Glass (1.59x).

Which is lighter, Glass or Plastic Polycarbonate?

Plastic Polycarbonate is lighter: 1,200 kg/m³ against 2,500 kg/m³ for Glass.

Which is stiffer, Glass or Plastic Polycarbonate?

Glass is stiffer: Young's modulus 72 GPa against 2.4 GPa for Plastic Polycarbonate, so the same part in Glass deflects less under the same load.

Which is lighter for the same job, Glass or Plastic Polycarbonate?

For the same stiffness or strength: Glass is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate; Plastic Polycarbonate is lighter for a strong rod or tie, strong beam, strong panel or plate.

Part that must beGlassPlastic Polycarbonate
Stiff rod or tie (tension)lighter14.4x heavier
Stiff beam (bending)lighter2.63x heavier
Stiff panel or platelighter49% heavier
Strong rod or tie3.3x heavierlighter
Strong beam2.83x heavierlighter
Strong panel or plate2.62x heavierlighter

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Thermal

Which conducts heat better, Glass or Plastic Polycarbonate?

Glass conducts heat better: 0.937 W/m·K against 0.2 W/m·K for Plastic Polycarbonate.

Which expands less with temperature?

Glass expands less: 8.3 µm/m·K against 65 µm/m·K for Plastic Polycarbonate.