Materials / Compare

Iron vs. Titanium Ti-6Al-4V

Compare Iron vs. Titanium Ti-6Al-4V strength, stiffness, weight and thermal properties.

IronWrought
Titanium Ti-6Al-4VWrought
MechanicalIronTitanium Ti-6Al-4V
Yield strength186MPa1885MPa24.76x stronger
Ultimate tensile strength290MPa1940MPa23.24x stronger
Elongation at break38%12.38x more ductile16%2
Young's modulus (stiffness)207GPa1107–122GPa3
Density7,860kg/m³14,430kg/m³21.77x lighter
Strength to weight23.7kN·m/kg200kN·m/kg8.44x higher
Stiffness to weight26.3MN·m/kg2% higher25.8MN·m/kg
Poisson's ratio0.28240.3422
Shear modulus80.7GPa1.89x stiffer in shear42.7GPa
Bulk modulus158GPa31% higher121GPa
Speed of sound5,132m/s5,084m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Brass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30IronTitanium Ti-6Al-4V
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Brass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30IronTitanium Ti-6Al-4V
Strength against densityHigher and further left: stronger for its weight
ThermalIronTitanium Ti-6Al-4V
Thermal conductivity73.2W/m·K111.1x more heat through a fin6.6W/m·K3
Thermal expansionmean13.7µm/m·K19µm/m·K31.52x less
100 mm part over a 50 °C swing68.5µm growth45µm growth1.52x less
Specific heat450J/kg·K1580J/kg·K329% higher
Heats up and cools (diffusivity)20.7mm²/s8.06x faster2.57mm²/s
Thermal shock resistance3,447W/m3,730W/m8% more resistant
Melting point1,532°C1melting range1,630–1,650°C2
Max service temperaturenot sourced400°C2
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Brass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30IronTitanium Ti-6Al-4V
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Brass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30IronTitanium Ti-6Al-4V
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources4 documents: Cleveland-Cliffs, TIMET, National Institute of Standards and Technology
Iron
Cleveland-Cliffs / AK Steel ARMCO Pure Iron Product Data Bulletin (07/2022): Table 1 typical physical properties, Table 2 typical mechanical properties after SRA/recrystallization anneal.
Titanium Ti-6Al-4V
TIMETAL 6-4 (Ti-6Al-4V Grade 5) annealed plate typical (TIMET properties manual) + TIMET datasheet TMC-0150 physical properties
  1. 1
    ARMCO Pure Iron Product Data Bulletin (2022)Cleveland-Cliffsarchived copyIron · Yield strength: typical (0.2% YS), hot rolled + SRA/recrystallization annealIron · Ultimate tensile strength: typical, SRA/recrystallization annealIron · Elongation at break: typical, gauge 4D0Iron · Young's modulus (stiffness): typical, after SRA/recrystallization annealIron · Density: typicalIron · Thermal conductivity: typical at 20 °CIron · Thermal expansion: mean, 20-399 °CIron · Specific heat: typicalIron · Melting point: typical
  2. 2
    TIMETAL 6-4 PropertiesTIMETarchived copyTitanium Ti-6Al-4V · Yield strength: typical, plate (>0.187 in), annealed, 0.2% offsetTitanium Ti-6Al-4V · Ultimate tensile strength: typical, plate, annealedTitanium Ti-6Al-4V · Elongation at break: typical, in 2 in., plate annealedTitanium Ti-6Al-4V · Density: nominalTitanium Ti-6Al-4V · Poisson's ratio: mean of TIMET measurementsTitanium Ti-6Al-4V · Melting point: melting rangeTitanium Ti-6Al-4V · Max service temperature: upper recommended use temperature
  3. 3
    TIMETAL 6-4 Data SheetTIMETarchived copyTitanium Ti-6Al-4V · Young's modulus (stiffness): typical range, 20 °CTitanium Ti-6Al-4V · Thermal conductivity: typical, 20 °C, mill annealedTitanium Ti-6Al-4V · Thermal expansion: typical, mean 0-100 °CTitanium Ti-6Al-4V · Specific heat: typical, 20 °C
  4. 4
    Elastic Properties of Metals and Alloys, I. Iron, Nickel, and Iron-Nickel Alloys, J. Phys. Chem. Ref. Data 2 (1973)National Institute of Standards and Technologyarchived copyIron · Poisson's ratio: NIST critically evaluated best value (polycrystalline iron)

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Questions

Mechanical

Is Iron stronger than Titanium Ti-6Al-4V?

Titanium Ti-6Al-4V is stronger: its yield strength is 885 MPa against 186 MPa for Iron (4.76x).

Which is lighter, Iron or Titanium Ti-6Al-4V?

Titanium Ti-6Al-4V is lighter: 4,430 kg/m³ against 7,860 kg/m³ for Iron.

Which is stiffer, Iron or Titanium Ti-6Al-4V?

Iron is stiffer: Young's modulus 207 GPa against 115 GPa for Titanium Ti-6Al-4V, so the same part in Iron deflects less under the same load.

Which is lighter for the same job, Iron or Titanium Ti-6Al-4V?

For the same stiffness or strength: Iron is lighter for a stiff rod or tie (tension); Titanium Ti-6Al-4V is lighter for a stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.

Part that must beIronTitanium Ti-6Al-4V
Stiff rod or tie (tension)lighter2% heavier
Stiff beam (bending)32% heavierlighter
Stiff panel or plate46% heavierlighter
Strong rod or tie8.44x heavierlighter
Strong beam5.02x heavierlighter
Strong panel or plate3.87x heavierlighter

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Iron or Titanium Ti-6Al-4V?

Iron stretches further before it breaks: 38% elongation at break against 16% for Titanium Ti-6Al-4V.

Thermal

Which conducts heat better, Iron or Titanium Ti-6Al-4V?

Iron conducts heat better: 73.2 W/m·K against 6.6 W/m·K for Titanium Ti-6Al-4V.

Which expands less with temperature?

Titanium Ti-6Al-4V expands less: 9 µm/m·K against 13.7 µm/m·K for Iron.

Related comparisons