Materials / Compare

Plywood vs. Titanium Ti-6Al-4V

Compare Plywood vs. Titanium Ti-6Al-4V strength, stiffness, weight and thermal properties.

Change either side
PlywoodNatural
Titanium Ti-6Al-4VWrought
Try it on a partA sample part to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Mechanical
Yield strengthnot given (tensile used)885MPasourcetypical, plate (>0.187 in), annealed, 0.2% offset
Ultimate tensile strength41.4MPasourcemodulus of rupture (no direct tensile value)940MPasourcetypical, plate, annealed
Flexural strength41.4MPasourcestatic bending MOR (Douglas-fir); range 33.72-42.61 across speciesnot sourced
Elongation at breaknot sourced16%sourcetypical, in 2 in., plate annealed
Young's modulus (stiffness)7.45GPasourcestatic bending MOE of the panel (Douglas-fir); range 6.96-8.55 across species107–122GPasourcetypical range, 20 °C
Densitynot sourced4,430kg/m³sourcenominal
Strength to weightnot sourced200kN·m/kg
Stiffness to weightnot sourced25.8MN·m/kg
Poisson's rationot sourced0.342sourcemean of TIMET measurements
Shear modulusnot sourced42.7GPa
Bulk modulusnot sourced121GPa
Speed of soundnot sourced5,084m/s
Thermal
Thermal conductivity0.12W/m·KsourceAPA-recommended design value (Douglas-fir plywood), as reported by FPL/ORNL6.6W/m·Ksourcetypical, 20 °C, mill annealed
Thermal expansion3.1–4.5µm/m·Ksourcebase material: solid wood parallel to grain, ovendry, range across species9µm/m·Ksourcetypical, mean 0-100 °C
100 mm part over a 50 °C swing19µm growth2.37x less45µm growth
Specific heat1,700J/kg·Ksourcebase material: solid wood (all species), 12% MC, 27 C580J/kg·Ksourcetypical, 20 °C
Heats up and cools (diffusivity)not sourced2.57mm²/s
Thermal shock resistancenot sourced3,730W/m
Melting pointnot sourced1,630–1,650°Csourcemelting range
Max service temperaturenot sourced400°Csourceupper recommended use temperature
Values forDouglas-fir plywood sheathing (construction plywood per PS 1), static bending properties from USDA FPL Wood Handbook FPL-GTR-282 Ch. 12 Table 12-2 (Biblis 2000)TIMETAL 6-4 (Ti-6Al-4V Grade 5) annealed plate typical (TIMET properties manual) + TIMET datasheet TMC-0150 physical properties

Every value links to the document that states it. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Questions

Is Plywood stronger than Titanium Ti-6Al-4V?

Titanium Ti-6Al-4V is stronger: its yield strength is 885 MPa against tensile strength 41.4 MPa for Plywood (21.4x).

Which is stiffer, Plywood or Titanium Ti-6Al-4V?

Titanium Ti-6Al-4V is stiffer: Young's modulus 115 GPa against 7.45 GPa for Plywood, so the same part in Titanium Ti-6Al-4V deflects less under the same load.

Which conducts heat better, Plywood or Titanium Ti-6Al-4V?

Titanium Ti-6Al-4V conducts heat better: 6.6 W/m·K against 0.12 W/m·K for Plywood.

Which expands less with temperature?

Plywood expands less: 3.8 µm/m·K against 9 µm/m·K for Titanium Ti-6Al-4V.

Among 59 materials

1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonAluminumSteelIronTitaniumSteel AISI 1018Stainless 304Stainless 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless 303Stainless 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Brass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelTitanium Ti-6Al-4V
Stiffness against density
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberAluminumSteelIronTitaniumSteel AISI 1018Stainless 304Stainless 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless 303Stainless 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Brass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickTitanium Ti-6Al-4V