Materials / Compare

Stainless Steel 303 vs. Titanium Ti-6Al-4V

Compare Stainless Steel 303 vs. Titanium Ti-6Al-4V strength, stiffness, weight and thermal properties.

Stainless Steel 303Wrought
Titanium Ti-6Al-4VWrought
MechanicalStainless Steel 303Titanium Ti-6Al-4V
Yield strengthOutokumpu typical275MPa1885MPa23.22x stronger
Ultimate tensile strengthOutokumpu typical585MPa1940MPa21.61x stronger
Elongation at breakOutokumpu typical35%12.19x more ductile16%2
Young's modulus (stiffness)at RT200GPa1107–122GPa3
Densityat RT7,900kg/m³14,430kg/m³21.78x lighter
Strength to weight34.8kN·m/kg200kN·m/kg5.74x higher
Stiffness to weight25.3MN·m/kg25.8MN·m/kg2% higher
Poisson's ratiodesign value0.340.3422
Shear modulus76.9GPa1.8x stiffer in shear42.7GPa
Bulk modulus167GPa38% higher121GPa
Speed of sound5,032m/s5,084m/s1% faster
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Brass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Stainless Steel 303Titanium Ti-6Al-4V
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Brass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Stainless Steel 303Titanium Ti-6Al-4V
Strength against densityHigher and further left: stronger for its weight
ThermalStainless Steel 303Titanium Ti-6Al-4V
Thermal conductivityat RT15W/m·K12.27x more heat through a fin6.6W/m·K3
Thermal expansionmean16µm/m·K19µm/m·K31.78x less
100 mm part over a 50 °C swing80µm growth45µm growth1.78x less
Specific heatat RT500J/kg·K1580J/kg·K316% higher
Heats up and cools (diffusivity)3.8mm²/s48% faster2.57mm²/s
Thermal shock resistance902W/m3,730W/m4.13x more resistant
Melting pointnot sourcedmelting range1,630–1,650°C2
Max service temperaturecontinuous871°C5400°C2
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Brass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Stainless Steel 303Titanium Ti-6Al-4V
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Brass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Stainless Steel 303Titanium Ti-6Al-4V
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources5 documents: Outokumpu, TIMET, Steel Construction Institute, Carpenter Technology
Stainless Steel 303
1.4305 / UNS S30300, Outokumpu typical values (hot rolled, solution annealed) from 'Steel Grades, Properties and Global Standards'; max service from Carpenter CarTech 303 datasheet
Titanium Ti-6Al-4V
TIMETAL 6-4 (Ti-6Al-4V Grade 5) annealed plate typical (TIMET properties manual) + TIMET datasheet TMC-0150 physical properties
  1. 1
    Steel Grades, Properties and Global StandardsOutokumpuarchived copyStainless Steel 303 · Yield strength: Outokumpu typical (product P = hot rolled plate, transverse)Stainless Steel 303 · Ultimate tensile strength: Outokumpu typicalStainless Steel 303 · Elongation at break: Outokumpu typical, A5Stainless Steel 303 · Young's modulus (stiffness): at RT (Table 12)Stainless Steel 303 · Density: at RTStainless Steel 303 · Thermal conductivity: at RTStainless Steel 303 · Thermal expansion: mean, 20–100 °CStainless Steel 303 · Specific heat: at RT
  2. 2
    TIMETAL 6-4 PropertiesTIMETarchived copyTitanium Ti-6Al-4V · Yield strength: typical, plate (>0.187 in), annealed, 0.2% offsetTitanium Ti-6Al-4V · Ultimate tensile strength: typical, plate, annealedTitanium Ti-6Al-4V · Elongation at break: typical, in 2 in., plate annealedTitanium Ti-6Al-4V · Density: nominalTitanium Ti-6Al-4V · Poisson's ratio: mean of TIMET measurementsTitanium Ti-6Al-4V · Melting point: melting rangeTitanium Ti-6Al-4V · Max service temperature: upper recommended use temperature
  3. 3
    TIMETAL 6-4 Data SheetTIMETarchived copyTitanium Ti-6Al-4V · Young's modulus (stiffness): typical range, 20 °CTitanium Ti-6Al-4V · Thermal conductivity: typical, 20 °C, mill annealedTitanium Ti-6Al-4V · Thermal expansion: typical, mean 0-100 °CTitanium Ti-6Al-4V · Specific heat: typical, 20 °C
  4. 4
    Design Manual for Structural Stainless Steel, 4th Edition (P413)Steel Construction Institutearchived copyStainless Steel 303 · Poisson's ratio: design value (structural stainless steels)
  5. 5
    Carpenter Stainless Type 303 Data SheetCarpenter Technologyarchived copyStainless Steel 303 · Max service temperature: continuous, scaling limit

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Questions

Mechanical

Is Stainless Steel 303 stronger than Titanium Ti-6Al-4V?

Titanium Ti-6Al-4V is stronger: its yield strength is 885 MPa against 275 MPa for Stainless Steel 303 (3.22x).

Which is lighter, Stainless Steel 303 or Titanium Ti-6Al-4V?

Titanium Ti-6Al-4V is lighter: 4,430 kg/m³ against 7,900 kg/m³ for Stainless Steel 303.

Which is stiffer, Stainless Steel 303 or Titanium Ti-6Al-4V?

Stainless Steel 303 is stiffer: Young's modulus 200 GPa against 115 GPa for Titanium Ti-6Al-4V, so the same part in Stainless Steel 303 deflects less under the same load.

Which is lighter for the same job, Stainless Steel 303 or Titanium Ti-6Al-4V?

For the same stiffness or strength: Titanium Ti-6Al-4V is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.

Part that must beStainless Steel 303Titanium Ti-6Al-4V
Stiff rod or tie (tension)2% heavierlighter
Stiff beam (bending)35% heavierlighter
Stiff panel or plate48% heavierlighter
Strong rod or tie5.74x heavierlighter
Strong beam3.89x heavierlighter
Strong panel or plate3.2x heavierlighter

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Stainless Steel 303 or Titanium Ti-6Al-4V?

Stainless Steel 303 stretches further before it breaks: 35% elongation at break against 16% for Titanium Ti-6Al-4V.

Thermal

Which conducts heat better, Stainless Steel 303 or Titanium Ti-6Al-4V?

Stainless Steel 303 conducts heat better: 15 W/m·K against 6.6 W/m·K for Titanium Ti-6Al-4V.

Which expands less with temperature?

Titanium Ti-6Al-4V expands less: 9 µm/m·K against 16 µm/m·K for Stainless Steel 303.