Materials / FDM

FDM ASA

FDM ASA strength, stiffness, density and thermal properties, with their source.

A bracket in FDM ASA, 3D-printed (layer lines) finish.

Process3D printed (FDM)
Mechanical
Yield strengthnot given (tensile used)
Ultimate tensile strength37MPasourcetypical
Flexural strength65MPasourcetypical
Elongation at break9.2%sourcetypical
Young's modulus (stiffness)2.45GPasourcetypical
Density1,050kg/m³sourcetypical
Strength to weight35.2kN·m/kg
Stiffness to weight2.33MN·m/kg
Poisson's rationot sourced
Shear modulusnot sourced
Bulk modulusnot sourced
Speed of sound1,528m/s
Thermal
Thermal conductivity0.17W/m·Ksourcebase material: INEOS Styrolution Luran S 777K injection-molding ASA, typical
Thermal expansion80–110µm/m·Ksourcebase material: INEOS Styrolution Luran S 777K injection-molding ASA, range
100 mm part over a 50 °C swing475µm growth
Specific heatnot sourced
Heats up and cools (diffusivity)not sourced
Thermal shock resistancenot sourced
Max service temperature92°CsourceHDT 1.8 MPa
Values forBambu Lab ASA, TDS V3.0, printed specimens X-Y; nozzle 260 °C, bed 80 °C, 200 mm/s, 100% infill; annealed and dried 80 °C for 12 h before testing.

FDM ASA is 3D printed: its properties depend on build direction and print settings; these are typical values.

Among 59 materials

1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelFDM ASA
Stiffness against density
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickFDM ASA
Strength against density

Compare FDM ASA with