Materials / Steel

Steel A992

Steel A992 (structural wide-flange) strength, stiffness, density and thermal properties, with their source.

A bracket in Steel A992, hot-rolled (mill scale) finish.

ProcessWrought
Mechanical
Yield strength385MPasourcetypical: mean of 20,295 A992 flange mill-test coupons (1998 SSPC survey), as reported by AISC
Ultimate tensile strength505MPasourcetypical: mean of 20,295 A992 flange mill-test coupons (1998 SSPC survey)
Elongation at breaknot sourced
Young's modulus (stiffness)200GPasourcedesign value (AISC 360-16)
Density7,850kg/m³sourcenominal (constructional data)
Strength to weight49kN·m/kg
Stiffness to weight25.5MN·m/kg
Poisson's ratio0.3sourcedesign value (AISC 360-16 Commentary)
Shear modulus76.9GPa
Bulk modulus167GPa
Speed of sound5,048m/s
Thermal
Thermal conductivity48W/m·Ksourcenominal at 20 °C
Thermal expansion12µm/m·Ksourcenominal (constructional data, no temperature range stated)
100 mm part over a 50 °C swing60µm growth
Specific heat460–480J/kg·Ksourcebase material: EN S275JR unalloyed structural steel (the EN counterpart of A36), typical, 50/100 °C
Heats up and cools (diffusivity)13mm²/s
Thermal shock resistance5,390W/m
Values forASTM A992 W-shapes; Fy/Fu specified minimums from AISC publications (AISC 360-16 Commentary; Modern Steel Construction); elastic constants AISC 360; physical constants from the bauforumstahl structural-steel EPD, which names A992 among covered product standards.

Among 59 materials

1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelSteel A992
Stiffness against density
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickSteel A992
Strength against density

Compare Steel A992 with