Materials / Aluminum

Aluminum 3003-O

Aluminum 3003-O (annealed tube, brazed fin) strength, stiffness, density and thermal properties, with their source.

A panel in Aluminum 3003-O, brushed finish.

Mechanical
Yield strength40MPa1
Ultimate tensile strength110MPa1
Elongation at break30%1
Young's modulus (stiffness)69GPa1
Density2,730kg/m³1
Strength to weight14.7kN·m/kg
Stiffness to weight25.3MN·m/kg
Poisson's rationot sourced
Shear modulusnot sourced
Bulk modulusnot sourced
Speed of sound5,027m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 3003-O
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 3003-O
Strength against densityHigher and further left: stronger for its weight
Thermal
Thermal conductivity193W/m·K1
Thermal expansion23.2µm/m·K1
100 mm part over a 50 °C swing116µm growth
Specific heatnot sourced
Heats up and cools (diffusivity)not sourced
Thermal shock resistancenot sourced
Melting pointmelting range640–655°C1
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 3003-O
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 3003-O
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Sources1 document: Kaiser Aluminum
Values for
Wrought. 3003-O (annealed) aluminium-manganese alloy, the heat-exchanger tube and brazing alloy, Kaiser Aluminum Tube & Pipe Alloy 3003 Technical Data (Rev. 05/06), typical properties; specific heat from the NIST cryogenic 3003-F fit at 293 K.
  1. 1
    Alloy 3003 Tube & Pipe Technical Data, Rev. 05/06Kaiser Aluminumarchived copyYield strength: typical, O, 0.0625 in specimenUltimate tensile strength: typical, OElongation at break: typical, O, in 4DYoung's modulus (stiffness): typicalDensity: nominal, 20 °CThermal conductivity: typical, O, 20 °CThermal expansion: typical, mean 20-100 °CMelting point: melting range

Thermal properties of Aluminum 3003-O

Thermal conductivity of Aluminum 3003-O

Aluminum 3003-O has a thermal conductivity of 193 W/m·K (112 BTU/hr·ft·°F). Basis: typical, O, 20 °C. Source: Kaiser Aluminum, Alloy 3003 Tube & Pipe Technical Data, Rev. 05/06archived copy.

Coefficient of thermal expansion of Aluminum 3003-O

Aluminum 3003-O expands 23.2 µm/m·K (12.9 µin/in·°F): a 100 mm part grows 116 µm over a 50 °C rise. Basis: typical, mean 20-100 °C. Source: Kaiser Aluminum, Alloy 3003 Tube & Pipe Technical Data, Rev. 05/06archived copy.

Melting point of Aluminum 3003-O

Aluminum 3003-O melts at 640–655 °C (1,184–1,211 °F). Basis: melting range. Source: Kaiser Aluminum, Alloy 3003 Tube & Pipe Technical Data, Rev. 05/06archived copy.

Compare Aluminum 3003-O with