Mechanical
Yield strengthnot given (tensile used)
Ultimate tensile strength5.1MPasourcemodulus of rupture (no direct tensile value)
Compressive strength77.9MPasourcemean unit compressive strength, solid extruded brick (survey mean; SD 30.8 MPa)
Elongation at breaknot sourced
Young's modulus (stiffness)not sourced
Density2,082kg/m³sourceface brick density row used for k (BIA notes most fired clay brick 120-130 lb/ft3)
Strength to weight2.45kN·m/kg
Stiffness to weightnot sourced
Poisson's rationot sourced
Shear modulusnot sourced
Bulk modulusnot sourced
Speed of soundnot sourced
Thermal
Thermal conductivity0.92–1.12W/m·Ksourcerange for 130 lb/ft3 face brick (ASHRAE 2013 via BIA)
Thermal expansion7.2µm/m·KsourceTMS Code average coefficient, clay/shale unit masonry
100 mm part over a 50 °C swing36µm growth
Specific heat837J/kg·Ksourcevalue used in BIA heat-capacity sample calculation
Heats up and cools (diffusivity)0.585mm²/s
Thermal shock resistancenot sourced
Values forSolid extruded clay/shale brick units (BIA 1993 manufacturer survey, TN 3A 2024); face brick of 130 lb/ft3 for thermal properties (BIA TN 4, from ASHRAE 2013); CTE is the TMS Code value for clay/shale masonry

Among 59 materials

1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonAluminumSteelIronTitaniumSteel AISI 1018Stainless 304Stainless 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless 303Stainless 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless Steel
Stiffness against density
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberAluminumSteelIronTitaniumSteel AISI 1018Stainless 304Stainless 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless 303Stainless 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrick
Strength against density

Compare Brick with