Materials / Compare

Aluminum 2024-T351 vs. Plastic TPU

Compare Aluminum 2024-T351 vs. Plastic TPU strength, stiffness, weight and thermal properties.

Aluminum 2024-T351Wrought
Plastic TPU3D printed (FDM)
MechanicalAluminum 2024-T351Plastic TPU
Yield strength324MPa1not given (tensile used)
Ultimate tensile strength469MPa123.7MPa2
Flexural strengthnot sourced4.1MPa2
Elongation at break19%1not sourced
Young's modulus (stiffness)73.1GPa11,091x stiffer0.067GPa2
Density2,770kg/m³11,220kg/m³22.27x lighter
Strength to weight117kN·m/kg6.02x higher19.4kN·m/kg
Stiffness to weight26.4MN·m/kg481x higher0.0549MN·m/kg
Poisson's ratio0.333not sourced
Shear modulus27.5GPanot sourced
Bulk modulus71.7GPanot sourced
Speed of sound5,137m/s21.9x faster234m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 2024-T351Plastic TPU
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 2024-T351Plastic TPU
Strength against densityHigher and further left: stronger for its weight
ThermalAluminum 2024-T351Plastic TPU
Thermal conductivity120W/m·K1not sourced
Thermal expansion22.9µm/m·K1not sourced
100 mm part over a 50 °C swing115µm growthnot sourced
Specific heat875J/kg·K1not sourced
Heats up and cools (diffusivity)49.5mm²/snot sourced
Thermal shock resistance15,561W/mnot sourced
Melting pointmelting range502–638°C1217°C2
Max service temperaturenot sourcedHDT 0.455 MPa50.3°C2
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 2024-T351
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 2024-T351
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources3 documents: Kaiser Aluminum, UltiMaker, U.S. Department of Defense
Aluminum 2024-T351
2024-T4/T351, Kaiser Aluminum sheet, coil & plate typical datasheet; Poisson from MIL-HDBK-5J
Plastic TPU
Ultimaker TPU 95A, 3D-printed specimens, XY (flat); Ultimaker S5 Pro, engineering intent profile, 0.15 mm layer height, AA 0.4 print core, 100% infill, Cura 4.9, printed one-at-a-time, conditioned >=24 h at room temperature. TDS (file v5.00), April 29, 2022.
  1. 1
    Alloy 2024 Sheet, Coil & Plate Technical DataKaiser Aluminumarchived copyAluminum 2024-T351 · Yield strength: typical, 0.2% offset, .500 in dia specimenAluminum 2024-T351 · Ultimate tensile strength: typicalAluminum 2024-T351 · Elongation at break: typical, in 4DAluminum 2024-T351 · Young's modulus (stiffness): typicalAluminum 2024-T351 · Density: nominalAluminum 2024-T351 · Thermal conductivity: typical, 20 °CAluminum 2024-T351 · Thermal expansion: typical, mean 20-100 °CAluminum 2024-T351 · Specific heat: typical, at 100 °CAluminum 2024-T351 · Melting point: melting range
  2. 2
    Ultimaker TPU 95A Technical Data Sheet, v5.00UltiMakerarchived copyPlastic TPU · Ultimate tensile strength: typical, stress at breakPlastic TPU · Flexural strength: typicalPlastic TPU · Young's modulus (stiffness): typicalPlastic TPU · Density: typicalPlastic TPU · Melting point: typicalPlastic TPU · Max service temperature: HDT 0.455 MPa (printed specimens)
  3. 3
    MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseAluminum 2024-T351 · Poisson's ratio: typical (handbook physical constant), all tempers

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Plastic TPU is 3D printed: its properties depend on build direction and print settings; these are typical values.

Questions

Mechanical

Is Aluminum 2024-T351 stronger than Plastic TPU?

Aluminum 2024-T351 is stronger: its yield strength is 324 MPa against tensile strength 23.7 MPa for Plastic TPU (13.7x).

Which is lighter, Aluminum 2024-T351 or Plastic TPU?

Plastic TPU is lighter: 1,220 kg/m³ against 2,770 kg/m³ for Aluminum 2024-T351.

Which is stiffer, Aluminum 2024-T351 or Plastic TPU?

Aluminum 2024-T351 is stiffer: Young's modulus 73.1 GPa against 0.067 GPa for Plastic TPU, so the same part in Aluminum 2024-T351 deflects less under the same load.

Which is lighter for the same job, Aluminum 2024-T351 or Plastic TPU?

For the same stiffness or strength: Aluminum 2024-T351 is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.

Part that must beAluminum 2024-T351Plastic TPU
Stiff rod or tie (tension)lighter481x heavier
Stiff beam (bending)lighter14.5x heavier
Stiff panel or platelighter4.53x heavier
Strong rod or tielighter6.02x heavier
Strong beamlighter2.52x heavier
Strong panel or platelighter1.63x heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).