Materials / Compare

Aluminum 2024-T351 vs. Stainless Steel 303

Compare Aluminum 2024-T351 vs. Stainless Steel 303 strength, stiffness, weight and thermal properties.

Aluminum 2024-T351Wrought
Stainless Steel 303Wrought
MechanicalAluminum 2024-T351Stainless Steel 303
Yield strength324MPa118% strongerOutokumpu typical275MPa2
Ultimate tensile strength469MPa1Outokumpu typical585MPa225% stronger
Elongation at break19%1Outokumpu typical35%21.84x more ductile
Young's modulus (stiffness)73.1GPa1at RT200GPa22.74x stiffer
Density2,770kg/m³12.85x lighterat RT7,900kg/m³2
Strength to weight117kN·m/kg3.36x higher34.8kN·m/kg
Stiffness to weight26.4MN·m/kg4% higher25.3MN·m/kg
Poisson's ratio0.333design value0.34
Shear modulus27.5GPa76.9GPa2.8x stiffer in shear
Bulk modulus71.7GPa167GPa2.33x higher
Speed of sound5,137m/s2% faster5,032m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 17-4PHAluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 2024-T351Stainless Steel 303
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 17-4PHAluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 2024-T351Stainless Steel 303
Strength against densityHigher and further left: stronger for its weight
ThermalAluminum 2024-T351Stainless Steel 303
Thermal conductivity120W/m·K18x more heat through a finat RT15W/m·K2
Thermal expansion22.9µm/m·K1mean16µm/m·K243% less
100 mm part over a 50 °C swing115µm growth80µm growth43% less
Specific heat875J/kg·K11.75x higherat RT500J/kg·K2
Heats up and cools (diffusivity)49.5mm²/s13x faster3.8mm²/s
Thermal shock resistance15,561W/m17.2x more resistant902W/m
Melting pointmelting range502–638°C1not sourced
Max service temperaturenot sourcedcontinuous871°C5
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 17-4PHAluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 2024-T351Stainless Steel 303
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 17-4PHAluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 2024-T351Stainless Steel 303
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources5 documents: Kaiser Aluminum, Outokumpu, U.S. Department of Defense, Steel Construction Institute, Carpenter Technology
Aluminum 2024-T351
2024-T4/T351, Kaiser Aluminum sheet, coil & plate typical datasheet; Poisson from MIL-HDBK-5J
Stainless Steel 303
1.4305 / UNS S30300, Outokumpu typical values (hot rolled, solution annealed) from 'Steel Grades, Properties and Global Standards'; max service from Carpenter CarTech 303 datasheet
  1. 1
    Alloy 2024 Sheet, Coil & Plate Technical DataKaiser Aluminumarchived copyAluminum 2024-T351 · Yield strength: typical, 0.2% offset, .500 in dia specimenAluminum 2024-T351 · Ultimate tensile strength: typicalAluminum 2024-T351 · Elongation at break: typical, in 4DAluminum 2024-T351 · Young's modulus (stiffness): typicalAluminum 2024-T351 · Density: nominalAluminum 2024-T351 · Thermal conductivity: typical, 20 °CAluminum 2024-T351 · Thermal expansion: typical, mean 20-100 °CAluminum 2024-T351 · Specific heat: typical, at 100 °CAluminum 2024-T351 · Melting point: melting range
  2. 2
    Steel Grades, Properties and Global StandardsOutokumpuarchived copyStainless Steel 303 · Yield strength: Outokumpu typical (product P = hot rolled plate, transverse)Stainless Steel 303 · Ultimate tensile strength: Outokumpu typicalStainless Steel 303 · Elongation at break: Outokumpu typical, A5Stainless Steel 303 · Young's modulus (stiffness): at RT (Table 12)Stainless Steel 303 · Density: at RTStainless Steel 303 · Thermal conductivity: at RTStainless Steel 303 · Thermal expansion: mean, 20–100 °CStainless Steel 303 · Specific heat: at RT
  3. 3
    MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseAluminum 2024-T351 · Poisson's ratio: typical (handbook physical constant), all tempers
  4. 4
    Design Manual for Structural Stainless Steel, 4th Edition (P413)Steel Construction Institutearchived copyStainless Steel 303 · Poisson's ratio: design value (structural stainless steels)
  5. 5
    Carpenter Stainless Type 303 Data SheetCarpenter Technologyarchived copyStainless Steel 303 · Max service temperature: continuous, scaling limit

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Questions

Mechanical

Is Aluminum 2024-T351 stronger than Stainless Steel 303?

Aluminum 2024-T351 is stronger: its yield strength is 324 MPa against 275 MPa for Stainless Steel 303 (18%).

Which is lighter, Aluminum 2024-T351 or Stainless Steel 303?

Aluminum 2024-T351 is lighter: 2,770 kg/m³ against 7,900 kg/m³ for Stainless Steel 303.

Which is stiffer, Aluminum 2024-T351 or Stainless Steel 303?

Stainless Steel 303 is stiffer: Young's modulus 200 GPa against 73.1 GPa for Aluminum 2024-T351, so the same part in Stainless Steel 303 deflects less under the same load.

Which is lighter for the same job, Aluminum 2024-T351 or Stainless Steel 303?

For the same stiffness or strength: Aluminum 2024-T351 is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.

Part that must beAluminum 2024-T351Stainless Steel 303
Stiff rod or tie (tension)lighter4% heavier
Stiff beam (bending)lighter1.72x heavier
Stiff panel or platelighter2.04x heavier
Strong rod or tielighter3.36x heavier
Strong beamlighter3.18x heavier
Strong panel or platelighter3.1x heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Aluminum 2024-T351 or Stainless Steel 303?

Stainless Steel 303 stretches further before it breaks: 35% elongation at break against 19% for Aluminum 2024-T351.

Thermal

Which conducts heat better, Aluminum 2024-T351 or Stainless Steel 303?

Aluminum 2024-T351 conducts heat better: 120 W/m·K against 15 W/m·K for Stainless Steel 303.

Which expands less with temperature?

Stainless Steel 303 expands less: 16 µm/m·K against 22.9 µm/m·K for Aluminum 2024-T351.