Materials / Compare

Aluminum 5052-H32 vs. Copper C110

Compare Aluminum 5052-H32 vs. Copper C110 strength, stiffness, weight and thermal properties.

Aluminum 5052-H32Wrought
Copper C110Wrought
MechanicalAluminum 5052-H32Copper C110
Yield strength195MPa12.83x stronger69MPa2
Ultimate tensile strength230MPa1221MPa2
Elongation at break12%155%24.58x more ductile
Young's modulus (stiffness)70GPa1117GPa21.67x stiffer
Density2,685kg/m³33.32x lighter8,913kg/m³2
Strength to weight72.6kN·m/kg9.38x higher7.74kN·m/kg
Stiffness to weight26.1MN·m/kg1.98x higher13.1MN·m/kg
Poisson's ratio0.3330.344
Shear modulus26.3GPa43.7GPa1.66x stiffer in shear
Bulk modulus68.6GPa122GPa1.78x higher
Speed of sound5,106m/s41% faster3,626m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 5052-H32Copper C110
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 5052-H32Copper C110
Strength against densityHigher and further left: stronger for its weight
ThermalAluminum 5052-H32Copper C110
Thermal conductivitybase material138W/m·K1391W/m·K22.83x more heat through a fin
Thermal expansion23.8µm/m·K116.9µm/m·K241% less
100 mm part over a 50 °C swing119µm growth84.5µm growth41% less
Specific heatat 100 °C963J/kg·K32.5x higher385J/kg·K2
Heats up and cools (diffusivity)53.4mm²/s114mm²/s2.13x faster
Thermal shock resistance10,822W/m20% more resistant8,992W/m
Melting pointmelting range605–650°C1solidus-liquidus1,065–1,083°C2
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 5052-H32Copper C110
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 5052-H32Copper C110
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources4 documents: Kaiser Aluminum, Copper Development Association, U.S. Department of Defense, Wieland
Aluminum 5052-H32
5052-H32, Kaiser Aluminum tube & pipe typical datasheet (mechanical, CTE, melting); MIL-HDBK-5J (Poisson, density, specific heat)
Copper C110
C11000 ETP copper, annealed to 0.050 mm grain size (OS050), 1 in. rod, copper.org typical values
  1. 1
    Alloy 5052 Tube & Pipe Technical DataKaiser Aluminumarchived copyAluminum 5052-H32 · Yield strength: typical, 0.2% offsetAluminum 5052-H32 · Ultimate tensile strength: typicalAluminum 5052-H32 · Elongation at break: typicalAluminum 5052-H32 · Young's modulus (stiffness): typicalAluminum 5052-H32 · Thermal conductivity: base material: 5052 in O temper (same alloy, annealed); Kaiser typicalAluminum 5052-H32 · Thermal expansion: typical, mean 20-100 °CAluminum 5052-H32 · Melting point: melting range
  2. 2
    C11000 Alloy (copper.org)Copper Development Associationarchived copyCopper C110 · Yield strength: typical, 0.5% extension under loadCopper C110 · Ultimate tensile strength: typicalCopper C110 · Elongation at break: typical, 1 in. rodCopper C110 · Young's modulus (stiffness): typicalCopper C110 · Density: nominalCopper C110 · Thermal conductivity: typical, 20 °CCopper C110 · Thermal expansion: typical, mean 20-100 °CCopper C110 · Specific heat: typical, 20 °CCopper C110 · Melting point: solidus-liquidus
  3. 3
    MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseAluminum 5052-H32 · Density: nominalAluminum 5052-H32 · Poisson's ratio: typical (handbook physical constant)Aluminum 5052-H32 · Specific heat: at 100 °C (212 °F); table covers O, H32, H34, H36, H38
  4. 4
    Wieland-K32 (Cu-ETP, C11000) Data SheetWielandarchived copyCopper C110 · Poisson's ratio: reference value at room temperature (Wieland-K32 = Cu-ETP = C11000, rolled products)

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Questions

Mechanical

Is Aluminum 5052-H32 stronger than Copper C110?

Aluminum 5052-H32 is stronger: its yield strength is 195 MPa against 69 MPa for Copper C110 (2.83x).

Which is lighter, Aluminum 5052-H32 or Copper C110?

Aluminum 5052-H32 is lighter: 2,685 kg/m³ against 8,913 kg/m³ for Copper C110.

Which is stiffer, Aluminum 5052-H32 or Copper C110?

Copper C110 is stiffer: Young's modulus 117 GPa against 70 GPa for Aluminum 5052-H32, so the same part in Copper C110 deflects less under the same load.

Which is lighter for the same job, Aluminum 5052-H32 or Copper C110?

For the same stiffness or strength: Aluminum 5052-H32 is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.

Part that must beAluminum 5052-H32Copper C110
Stiff rod or tie (tension)lighter1.98x heavier
Stiff beam (bending)lighter2.57x heavier
Stiff panel or platelighter2.8x heavier
Strong rod or tielighter9.38x heavier
Strong beamlighter6.64x heavier
Strong panel or platelighter5.58x heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Aluminum 5052-H32 or Copper C110?

Copper C110 stretches further before it breaks: 55% elongation at break against 12% for Aluminum 5052-H32.

Thermal

Which conducts heat better, Aluminum 5052-H32 or Copper C110?

Copper C110 conducts heat better: 391 W/m·K against 138 W/m·K for Aluminum 5052-H32.

Which expands less with temperature?

Copper C110 expands less: 16.9 µm/m·K against 23.8 µm/m·K for Aluminum 5052-H32.

Related comparisons