Materials / Compare

Aluminum 5052-H32 vs. FDM PAHT-CF

Compare Aluminum 5052-H32 vs. FDM PAHT-CF strength, stiffness, weight and thermal properties.

Aluminum 5052-H32Wrought
FDM PAHT-CF3D printed (FDM)
MechanicalAluminum 5052-H32FDM PAHT-CF
Yield strength195MPa1not given (tensile used)
Ultimate tensile strength230MPa12.5x stronger92MPa2
Flexural strengthnot sourced125MPa2
Elongation at break12%143% more ductile8.4%2
Young's modulus (stiffness)70GPa118.1x stiffer3.86GPa2
Density2,685kg/m³31,060kg/m³22.53x lighter
Strength to weight72.6kN·m/kg86.8kN·m/kg20% higher
Stiffness to weight26.1MN·m/kg7.16x higher3.64MN·m/kg
Poisson's ratio0.333not sourced
Shear modulus26.3GPanot sourced
Bulk modulus68.6GPanot sourced
Speed of sound5,106m/s2.68x faster1,908m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 5052-H32FDM PAHT-CF
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 5052-H32FDM PAHT-CF
Strength against densityHigher and further left: stronger for its weight
ThermalAluminum 5052-H32FDM PAHT-CF
Thermal conductivitybase material138W/m·K1not sourced
Thermal expansion23.8µm/m·K1not sourced
100 mm part over a 50 °C swing119µm growthnot sourced
Specific heatat 100 °C963J/kg·K3not sourced
Heats up and cools (diffusivity)53.4mm²/snot sourced
Thermal shock resistance10,822W/mnot sourced
Melting pointmelting range605–650°C1225°C2
Glass transitionnot sourced70°C2
Max service temperaturenot sourcedHDT 1.8 MPa170°C2
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 5052-H32
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 5052-H32
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources3 documents: Kaiser Aluminum, Bambu Lab, U.S. Department of Defense
Aluminum 5052-H32
5052-H32, Kaiser Aluminum tube & pipe typical datasheet (mechanical, CTE, melting); MIL-HDBK-5J (Poisson, density, specific heat)
FDM PAHT-CF
Bambu Lab PAHT-CF, TDS V3.0, printed specimens X-Y, dry state; nozzle 290 °C, bed 100 °C, 100 mm/s, 100% infill; annealed and dried 80 °C for 12 h before testing.
  1. 1
    Alloy 5052 Tube & Pipe Technical DataKaiser Aluminumarchived copyAluminum 5052-H32 · Yield strength: typical, 0.2% offsetAluminum 5052-H32 · Ultimate tensile strength: typicalAluminum 5052-H32 · Elongation at break: typicalAluminum 5052-H32 · Young's modulus (stiffness): typicalAluminum 5052-H32 · Thermal conductivity: base material: 5052 in O temper (same alloy, annealed); Kaiser typicalAluminum 5052-H32 · Thermal expansion: typical, mean 20-100 °CAluminum 5052-H32 · Melting point: melting range
  2. 2
    Bambu PAHT-CF Technical Data Sheet, V3.0Bambu LabFDM PAHT-CF · Ultimate tensile strength: typicalFDM PAHT-CF · Flexural strength: typicalFDM PAHT-CF · Elongation at break: typicalFDM PAHT-CF · Young's modulus (stiffness): typicalFDM PAHT-CF · Density: typicalFDM PAHT-CF · Melting point: typicalFDM PAHT-CF · Glass transition: typicalFDM PAHT-CF · Max service temperature: HDT 1.8 MPa
  3. 3
    MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseAluminum 5052-H32 · Density: nominalAluminum 5052-H32 · Poisson's ratio: typical (handbook physical constant)Aluminum 5052-H32 · Specific heat: at 100 °C (212 °F); table covers O, H32, H34, H36, H38

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

FDM PAHT-CF is 3D printed: its properties depend on build direction and print settings; these are typical values.

Questions

Mechanical

Is Aluminum 5052-H32 stronger than FDM PAHT-CF?

Aluminum 5052-H32 is stronger: its yield strength is 195 MPa against tensile strength 92 MPa for FDM PAHT-CF (2.12x).

Which is lighter, Aluminum 5052-H32 or FDM PAHT-CF?

FDM PAHT-CF is lighter: 1,060 kg/m³ against 2,685 kg/m³ for Aluminum 5052-H32.

Which is stiffer, Aluminum 5052-H32 or FDM PAHT-CF?

Aluminum 5052-H32 is stiffer: Young's modulus 70 GPa against 3.86 GPa for FDM PAHT-CF, so the same part in Aluminum 5052-H32 deflects less under the same load.

Which is lighter for the same job, Aluminum 5052-H32 or FDM PAHT-CF?

For the same stiffness or strength: Aluminum 5052-H32 is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate; FDM PAHT-CF is lighter for a strong rod or tie, strong beam, strong panel or plate.

Part that must beAluminum 5052-H32FDM PAHT-CF
Stiff rod or tie (tension)lighter7.16x heavier
Stiff beam (bending)lighter1.68x heavier
Stiff panel or platelighter4% heavier
Strong rod or tie20% heavierlighter
Strong beam1.54x heavierlighter
Strong panel or plate1.74x heavierlighter

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Aluminum 5052-H32 or FDM PAHT-CF?

Aluminum 5052-H32 stretches further before it breaks: 12% elongation at break against 8.4% for FDM PAHT-CF.

Related comparisons