Materials / Compare

Aluminum 6063-T6 vs. Steel AISI 1018

Compare Aluminum 6063-T6 vs. Steel AISI 1018 strength, stiffness, weight and thermal properties.

Aluminum 6063-T6Wrought
Steel AISI 1018Wrought
MechanicalAluminum 6063-T6Steel AISI 1018
Yield strength215MPa1producer-stated372MPa21.73x stronger
Ultimate tensile strength240MPa1producer-stated441MPa21.84x stronger
Elongation at break12%1in 2 in15%225% more ductile
Young's modulus (stiffness)69GPa1base material200GPa3
Density2,700kg/m³1base material7,861kg/m³3
Strength to weight79.6kN·m/kg1.68x higher47.3kN·m/kg
Stiffness to weight25.6MN·m/kg25.4MN·m/kg
Poisson's rationot sourcedbase material0.323
Shear modulusnot sourced75.7GPa
Bulk modulusnot sourced185GPa
Speed of sound5,055m/s5,043m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumStainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 6063-T6Steel AISI 1018
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumStainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 6063-T6Steel AISI 1018
Strength against densityHigher and further left: stronger for its weight
ThermalAluminum 6063-T6Steel AISI 1018
Thermal conductivity201W/m·K1base material51.9W/m·K3
Thermal expansion23.4µm/m·K1base material12µm/m·K41.95x less
100 mm part over a 50 °C swing117µm growth60µm growth1.95x less
Specific heat901J/kg·K5base material486J/kg·K3
Heats up and cools (diffusivity)82.6mm²/s6.08x faster13.6mm²/s
Thermal shock resistancenot sourced5,473W/m
Melting pointmelting range615–655°C1not sourced
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumStainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 6063-T6Steel AISI 1018
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumStainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 6063-T6Steel AISI 1018
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources5 documents: Kaiser Aluminum, Niagara LaSalle, U.S. Department of Defense, Ovako, Hydro
Aluminum 6063-T6
6063-T6 extruded tube, Kaiser Aluminum Tube & Pipe Alloy 6063 Technical Data (Rev. 05/06), typical properties; specific heat from Hydro EN AW-6063 extruded-products datasheet (Rev.4, 03/2023).
Steel AISI 1018
AISI 1018 cold drawn bar (Niagara LaSalle, cold-finished bar producer)
  1. 1
    Alloy 6063 Tube & Pipe Technical Data, Rev. 05/06Kaiser Aluminumarchived copyAluminum 6063-T6 · Yield strength: typical, T6, 0.0625 in specimenAluminum 6063-T6 · Ultimate tensile strength: typical, T6Aluminum 6063-T6 · Elongation at break: typical, T6, in 4DAluminum 6063-T6 · Young's modulus (stiffness): typicalAluminum 6063-T6 · Density: nominal, 20 °CAluminum 6063-T6 · Thermal conductivity: typical, T6, 20 °CAluminum 6063-T6 · Thermal expansion: typical, mean 20-100 °CAluminum 6063-T6 · Melting point: melting range
  2. 2
    1018 PropertiesNiagara LaSallearchived copySteel AISI 1018 · Yield strength: producer-stated, cold drawnSteel AISI 1018 · Ultimate tensile strength: producer-stated, cold drawnSteel AISI 1018 · Elongation at break: in 2 in (50.8 mm)
  3. 3
    MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseSteel AISI 1018 · Young's modulus (stiffness): base material: AISI 1025 plain carbon steel (MIL-HDBK-5J design value; ASTM A108 bar is the cold-finished carbon-steel bar spec that also covers 1018)Steel AISI 1018 · Density: base material: AISI 1025 plain carbon steel (MIL-HDBK-5J design value; ASTM A108 bar is the cold-finished carbon-steel bar spec that also covers 1018)Steel AISI 1018 · Poisson's ratio: base material: AISI 1025 plain carbon steel (MIL-HDBK-5J design value; ASTM A108 bar is the cold-finished carbon-steel bar spec that also covers 1018)Steel AISI 1018 · Thermal conductivity: base material: AISI 1025 plain carbon steel (MIL-HDBK-5J design value; ASTM A108 bar is the cold-finished carbon-steel bar spec that also covers 1018)Steel AISI 1018 · Specific heat: base material: AISI 1025 plain carbon steel (MIL-HDBK-5J design value; ASTM A108 bar is the cold-finished carbon-steel bar spec that also covers 1018)
  4. 4
    S275JR Steel GradeOvakoSteel AISI 1018 · Thermal expansion: base material: unalloyed carbon steel, Ovako family table (S275JR, 'none alloyed structural steels', C <= 0.21%); mean 20-300 °C
  5. 5
    Technical Datasheet, Extruded Products: Alloy EN AW-6063 (Rev. 4, 2023)Hydroarchived copyAluminum 6063-T6 · Specific heat: typical, 20 °C (Hydro EN AW-6063)

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Questions

Mechanical

Is Aluminum 6063-T6 stronger than Steel AISI 1018?

Steel AISI 1018 is stronger: its yield strength is 372 MPa against 215 MPa for Aluminum 6063-T6 (1.73x).

Which is lighter, Aluminum 6063-T6 or Steel AISI 1018?

Aluminum 6063-T6 is lighter: 2,700 kg/m³ against 7,861 kg/m³ for Steel AISI 1018.

Which is stiffer, Aluminum 6063-T6 or Steel AISI 1018?

Steel AISI 1018 is stiffer: Young's modulus 200 GPa against 69 GPa for Aluminum 6063-T6, so the same part in Steel AISI 1018 deflects less under the same load.

Which is lighter for the same job, Aluminum 6063-T6 or Steel AISI 1018?

For the same stiffness or strength: Aluminum 6063-T6 is lighter for a stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.

Part that must beAluminum 6063-T6Steel AISI 1018
Stiff rod or tie (tension)about equalabout equal
Stiff beam (bending)lighter1.71x heavier
Stiff panel or platelighter2.04x heavier
Strong rod or tielighter1.68x heavier
Strong beamlighter2.02x heavier
Strong panel or platelighter2.21x heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Aluminum 6063-T6 or Steel AISI 1018?

Steel AISI 1018 stretches further before it breaks: 15% elongation at break against 12% for Aluminum 6063-T6.

Thermal

Which conducts heat better, Aluminum 6063-T6 or Steel AISI 1018?

Aluminum 6063-T6 conducts heat better: 201 W/m·K against 51.9 W/m·K for Steel AISI 1018.

Which expands less with temperature?

Steel AISI 1018 expands less: 12 µm/m·K against 23.4 µm/m·K for Aluminum 6063-T6.

Related comparisons