Materials / Compare

Aluminum 7075-T6 vs. Plastic Polycarbonate

Compare Aluminum 7075-T6 vs. Plastic Polycarbonate strength, stiffness, weight and thermal properties.

Aluminum 7075-T6Wrought
Plastic PolycarbonateBulk polymer (molded or machined)
MechanicalAluminum 7075-T6Plastic Polycarbonate
Yield strength503MPa17.74x stronger65MPa2
Ultimate tensile strength572MPa165MPa2
Flexural strengthnot sourced97MPa2
Elongation at break11%1125%211.4x more ductile
Young's modulus (stiffness)71GPa129.6x stiffer2.4GPa2
Density2,800kg/m³31,200kg/m³22.33x lighter
Strength to weight180kN·m/kg3.32x higher54.2kN·m/kg
Stiffness to weight25.4MN·m/kg12.7x higher2MN·m/kg
Poisson's ratio0.3340.385
Shear modulus26.7GPa30.7x stiffer in shear0.87GPa
Bulk modulus69.6GPa20.9x higher3.33GPa
Speed of sound5,036m/s3.56x faster1,414m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7075-T6Plastic Polycarbonate
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7075-T6Plastic Polycarbonate
Strength against densityHigher and further left: stronger for its weight
ThermalAluminum 7075-T6Plastic Polycarbonate
Thermal conductivity130W/m·K3650x more heat through a fin0.2W/m·K2
Thermal expansion23.4µm/m·K32.78x less65µm/m·K2
100 mm part over a 50 °C swing117µm growth2.78x less325µm growth
Specific heat960J/kg·K31,172J/kg·K622% higher
Heats up and cools (diffusivity)48.4mm²/s340x faster0.142mm²/s
Thermal shock resistance26,370W/m510x more resistant51.7W/m
Melting pointmelting range532–635°C3not sourced
Glass transitionnot sourced144°C2
Max service temperaturenot sourcedUL 746B RTI125°C2
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7075-T6Plastic Polycarbonate
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7075-T6Plastic Polycarbonate
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources6 documents: Kaiser Aluminum, Covestro, U.S. Department of Defense, Bayer MaterialScience
Aluminum 7075-T6
7075-T6/T651, Kaiser Aluminum rod & bar (mechanical) and sheet/coil/plate (physical) typical datasheets; Poisson from MIL-HDBK-5J
Plastic Polycarbonate
Covestro Makrolon 2405 general-purpose PC (MVR 19), Covestro technical datasheet version 2026-09-28, typical values
  1. 1
    Alloy 7075 Rod & Bar Technical DataKaiser Aluminumarchived copyAluminum 7075-T6 · Yield strength: typical, 0.2% offset, .500 in dia specimenAluminum 7075-T6 · Ultimate tensile strength: typicalAluminum 7075-T6 · Elongation at break: typical, in 4DAluminum 7075-T6 · Young's modulus (stiffness): typical
  2. 2
    Makrolon 2405 Technical Data SheetCovestroPlastic Polycarbonate · Yield strength: typical, tensile yieldPlastic Polycarbonate · Ultimate tensile strength: typical, stress at breakPlastic Polycarbonate · Flexural strength: typical, flexural strengthPlastic Polycarbonate · Elongation at break: typical, strain at breakPlastic Polycarbonate · Young's modulus (stiffness): typicalPlastic Polycarbonate · Density: typicalPlastic Polycarbonate · Thermal conductivity: typical, through-plane, 23 CPlastic Polycarbonate · Thermal expansion: typical, 23-55 C, parallel and normalPlastic Polycarbonate · Glass transition: typical, DSC 10 C/minPlastic Polycarbonate · Max service temperature: UL 746B RTI, tensile strength, 1.5 mm
  3. 3
    Alloy 7075 Sheet, Coil & Plate Technical DataKaiser Aluminumarchived copyAluminum 7075-T6 · Density: nominalAluminum 7075-T6 · Thermal conductivity: typical, 20 °C, T651Aluminum 7075-T6 · Thermal expansion: typical, mean 20-100 °CAluminum 7075-T6 · Specific heat: typical, at 100 °CAluminum 7075-T6 · Melting point: melting range
  4. 4
    MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseAluminum 7075-T6 · Poisson's ratio: typical (handbook physical constant)
  5. 5
    Engineering Polymers Part and Mold Design: Thermoplastics, A Design GuideCovestroarchived copyPlastic Polycarbonate · Poisson's ratio: typical, polycarbonate family (Covestro Part and Mold Design guide, Table 3-1)
  6. 6
    Makrolon 2405 Data Sheet, ASTM valuesBayer MaterialSciencearchived copyPlastic Polycarbonate · Specific heat: typical (guide value), Bayer ASTM datasheet for Makrolon 2405, ASTM D 2766

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Questions

Mechanical

Is Aluminum 7075-T6 stronger than Plastic Polycarbonate?

Aluminum 7075-T6 is stronger: its yield strength is 503 MPa against 65 MPa for Plastic Polycarbonate (7.74x).

Which is lighter, Aluminum 7075-T6 or Plastic Polycarbonate?

Plastic Polycarbonate is lighter: 1,200 kg/m³ against 2,800 kg/m³ for Aluminum 7075-T6.

Which is stiffer, Aluminum 7075-T6 or Plastic Polycarbonate?

Aluminum 7075-T6 is stiffer: Young's modulus 71 GPa against 2.4 GPa for Plastic Polycarbonate, so the same part in Aluminum 7075-T6 deflects less under the same load.

Which is lighter for the same job, Aluminum 7075-T6 or Plastic Polycarbonate?

For the same stiffness or strength: Aluminum 7075-T6 is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.

Part that must beAluminum 7075-T6Plastic Polycarbonate
Stiff rod or tie (tension)lighter12.7x heavier
Stiff beam (bending)lighter2.33x heavier
Stiff panel or platelighter33% heavier
Strong rod or tielighter3.32x heavier
Strong beamlighter1.68x heavier
Strong panel or platelighter19% heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Aluminum 7075-T6 or Plastic Polycarbonate?

Plastic Polycarbonate stretches further before it breaks: 125% elongation at break against 11% for Aluminum 7075-T6.

Thermal

Which conducts heat better, Aluminum 7075-T6 or Plastic Polycarbonate?

Aluminum 7075-T6 conducts heat better: 130 W/m·K against 0.2 W/m·K for Plastic Polycarbonate.

Which expands less with temperature?

Aluminum 7075-T6 expands less: 23.4 µm/m·K against 65 µm/m·K for Plastic Polycarbonate.