Materials / Compare

Brass C360 vs. Plastic Polypropylene

Compare Brass C360 vs. Plastic Polypropylene strength, stiffness, weight and thermal properties.

Brass C360Wrought
Plastic PolypropyleneBulk polymer (molded or machined)
MechanicalBrass C360Plastic Polypropylene
Yield strength310MPa19.39x stronger33MPa2
Ultimate tensile strength400MPa1not stated (yield given)
Elongation at break25%1not sourced
Young's modulus (stiffness)96.5GPa166.6x stiffer1.45GPa2
Density8,498kg/m³1900kg/m³29.44x lighter
Strength to weight36.5kN·m/kg36.7kN·m/kg
Stiffness to weight11.4MN·m/kg7.05x higher1.61MN·m/kg
Poisson's ratiobase material0.343base material0.424
Shear modulus36GPa70.5x stiffer in shear0.511GPa
Bulk modulus101GPa33.3x higher3.02GPa
Speed of sound3,370m/s2.65x faster1,269m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Brass C360Plastic Polypropylene
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Brass C360Plastic Polypropylene
Strength against densityHigher and further left: stronger for its weight
ThermalBrass C360Plastic Polypropylene
Thermal conductivity116W/m·K1base material0.17–0.22W/m·K4
Thermal expansion20.5µm/m·K1base material80–100µm/m·K4
100 mm part over a 50 °C swing103µm growth4.39x less450µm growth
Specific heat377J/kg·K1not sourced
Heats up and cools (diffusivity)36.2mm²/snot sourced
Thermal shock resistance11,997W/m419x more resistant28.6W/m
Melting pointsolidus-liquidus888–899°C1not sourced
Max service temperaturenot sourcedHDT 0.45 MPa90°C2
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Brass C360Plastic Polypropylene
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Brass C360Plastic Polypropylene
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources4 documents: Copper Development Association, LyondellBasell, Wieland, INEOS Olefins & Polymers USA
Brass C360
C36000 free-cutting brass, H02 half-hard rod 1 in. section (20% cold work), copper.org typical values
Plastic Polypropylene
LyondellBasell Moplen HP501H polypropylene homopolymer (general purpose), typical ISO values
  1. 1
    C36000 Alloy (copper.org)Copper Development Associationarchived copyBrass C360 · Yield strength: typical, 0.5% extension under loadBrass C360 · Ultimate tensile strength: typicalBrass C360 · Elongation at break: typical, 1 in. rodBrass C360 · Young's modulus (stiffness): typical, temper-independentBrass C360 · Density: nominalBrass C360 · Thermal conductivity: typical, 20 °CBrass C360 · Thermal expansion: typical, mean 20-300 °CBrass C360 · Specific heat: typical, 20 °CBrass C360 · Melting point: solidus-liquidus
  2. 2
    Moplen HP501H Product DataLyondellBasellPlastic Polypropylene · Yield strength: typical, tensile stress at yield ISO 527Plastic Polypropylene · Young's modulus (stiffness): typical, tensile modulus ISO 527Plastic Polypropylene · Density: typical, 23 °C ISO 1183-1Plastic Polypropylene · Max service temperature: HDT 0.45 MPa (ISO 75B), unannealed
  3. 3
    Wieland-Z30 (CuZn39Pb2, C37700) Data SheetWielandarchived copyBrass C360 · Poisson's ratio: base material: leaded free-machining brass CuZn39Pb2 (C37700), Wieland-Z30 rolled products, reference value at room temperature
  4. 4
    Typical Engineering Properties of PolypropyleneINEOS Olefins & Polymers USAarchived copyPlastic Polypropylene · Poisson's ratio: base material: polypropylene homopolymer family (INEOS Olefins & Polymers USA, Typical Engineering Properties of Polypropylene)Plastic Polypropylene · Thermal conductivity: base material: polypropylene homopolymer family (INEOS Olefins & Polymers USA, Typical Engineering Properties of Polypropylene)Plastic Polypropylene · Thermal expansion: base material: polypropylene homopolymer family (INEOS Olefins & Polymers USA, Typical Engineering Properties of Polypropylene)

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Questions

Mechanical

Is Brass C360 stronger than Plastic Polypropylene?

Brass C360 is stronger: its yield strength is 310 MPa against 33 MPa for Plastic Polypropylene (9.39x).

Which is lighter, Brass C360 or Plastic Polypropylene?

Plastic Polypropylene is lighter: 900 kg/m³ against 8,498 kg/m³ for Brass C360.

Which is stiffer, Brass C360 or Plastic Polypropylene?

Brass C360 is stiffer: Young's modulus 96.5 GPa against 1.45 GPa for Plastic Polypropylene, so the same part in Brass C360 deflects less under the same load.

Which is lighter for the same job, Brass C360 or Plastic Polypropylene?

For the same stiffness or strength: Brass C360 is lighter for a stiff rod or tie (tension); Plastic Polypropylene is lighter for a stiff beam (bending), stiff panel or plate, strong beam, strong panel or plate.

Part that must beBrass C360Plastic Polypropylene
Stiff rod or tie (tension)lighter7.05x heavier
Stiff beam (bending)16% heavierlighter
Stiff panel or plate2.33x heavierlighter
Strong rod or tieabout equalabout equal
Strong beam2.12x heavierlighter
Strong panel or plate3.08x heavierlighter

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Thermal

Which conducts heat better, Brass C360 or Plastic Polypropylene?

Brass C360 conducts heat better: 116 W/m·K against 0.195 W/m·K for Plastic Polypropylene.

Which expands less with temperature?

Brass C360 expands less: 20.5 µm/m·K against 90 µm/m·K for Plastic Polypropylene.

Related comparisons