Materials / Compare
Brass C360 vs. Stainless Steel 303
Compare Brass C360 vs. Stainless Steel 303 strength, stiffness, weight and thermal properties.
| Try it on a partA bracket to run stress or thermal on, free in your browser | Open in LessCAD | Open in LessCAD |
|---|---|---|
| Mechanical | ||
| Yield strength | 310MPasourcetypical, 0.5% extension under load | 275MPasourceOutokumpu typical (product P = hot rolled plate, transverse) |
| Ultimate tensile strength | 400MPasourcetypical | 585MPasourceOutokumpu typical |
| Elongation at break | 25%sourcetypical, 1 in. rod | 35%sourceOutokumpu typical, A5 |
| Young's modulus (stiffness) | 96.5GPasourcetypical, temper-independent | 200GPasourceat RT (Table 12) |
| Density | 8,498kg/m³sourcenominal | 7,900kg/m³sourceat RT |
| Strength to weight | 36.5kN·m/kg5% higher | 34.8kN·m/kg |
| Stiffness to weight | 11.4MN·m/kg | 25.3MN·m/kg2.23x higher |
| Poisson's ratio | 0.34sourcebase material: leaded free-machining brass CuZn39Pb2 (C37700), Wieland-Z30 rolled products, reference value at room temperature | 0.3sourcedesign value (structural stainless steels) |
| Shear modulus | 36GPa | 76.9GPa2.14x stiffer in shear |
| Bulk modulus | 101GPa | 167GPa |
| Speed of sound | 3,370m/s | 5,032m/s |
| Thermal | ||
| Thermal conductivity | 116W/m·Ksourcetypical, 20 °C | 15W/m·Ksourceat RT |
| Thermal expansion | 20.5µm/m·Ksourcetypical, mean 20-300 °C | 16µm/m·Ksourcemean, 20–100 °C |
| 100 mm part over a 50 °C swing | 103µm growth | 80µm growth28% less |
| Specific heat | 377J/kg·Ksourcetypical, 20 °C | 500J/kg·Ksourceat RT |
| Heats up and cools (diffusivity) | 36.2mm²/s9.54x faster | 3.8mm²/s |
| Thermal shock resistance | 11,997W/m13.3x more resistant | 902W/m |
| Melting point | 888–899°Csourcesolidus-liquidus | not sourced |
| Max service temperature | not sourced | 871°Csourcecontinuous, scaling limit |
| Values for | C36000 free-cutting brass, H02 half-hard rod 1 in. section (20% cold work), copper.org typical values | 1.4305 / UNS S30300, Outokumpu typical values (hot rolled, solution annealed) from 'Steel Grades, Properties and Global Standards'; max service from Carpenter CarTech 303 datasheet |
Every value links to the document that states it. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.
Questions
Is Brass C360 stronger than Stainless Steel 303?
Brass C360 is stronger: its yield strength is 310 MPa against 275 MPa for Stainless Steel 303 (13%).
Which is lighter, Brass C360 or Stainless Steel 303?
Stainless Steel 303 is lighter: 7,900 kg/m³ against 8,498 kg/m³ for Brass C360.
Which is stiffer, Brass C360 or Stainless Steel 303?
Stainless Steel 303 is stiffer: Young's modulus 200 GPa against 96.5 GPa for Brass C360, so the same part in Stainless Steel 303 deflects less under the same load.
Which is lighter for the same job, Brass C360 or Stainless Steel 303?
For the same stiffness or strength: Brass C360 is lighter for a strong rod or tie; Stainless Steel 303 is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong panel or plate.
| Part that must be | Brass C360 | Stainless Steel 303 |
|---|---|---|
| Stiff rod or tie (tension) | 2.23x heavier | lighter |
| Stiff beam (bending) | 1.55x heavier | lighter |
| Stiff panel or plate | 37% heavier | lighter |
| Strong rod or tie | lighter | 5% heavier |
| Strong beam | about equal | about equal |
| Strong panel or plate | 1% heavier | lighter |
For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).
Which conducts heat better, Brass C360 or Stainless Steel 303?
Brass C360 conducts heat better: 116 W/m·K against 15 W/m·K for Stainless Steel 303.
Which expands less with temperature?
Stainless Steel 303 expands less: 16 µm/m·K against 20.5 µm/m·K for Brass C360.