Materials / Compare
Brass C360 vs. Stainless Steel 316
Compare Brass C360 vs. Stainless Steel 316 strength, stiffness, weight and thermal properties.
| Try it on a partA bracket to run stress or thermal on, free in your browser | Open in LessCAD | Open in LessCAD |
|---|---|---|
| Mechanical | ||
| Yield strength | 310MPasourcetypical, 0.5% extension under load | 265MPasourcetypical (representative), annealed 1.0 mm sheet |
| Ultimate tensile strength | 400MPasourcetypical | 583MPasourcetypical (representative), annealed 1.0 mm sheet |
| Elongation at break | 25%sourcetypical, 1 in. rod | 61%sourcetypical (representative), annealed, in 2 in. (51 mm) |
| Young's modulus (stiffness) | 96.5GPasourcetypical, temper-independent | 200GPasourcetypical, in tension |
| Density | 8,498kg/m³sourcenominal | 8,027kg/m³sourcetypical |
| Strength to weight | 36.5kN·m/kg10% higher | 33kN·m/kg |
| Stiffness to weight | 11.4MN·m/kg | 24.9MN·m/kg2.19x higher |
| Poisson's ratio | 0.34sourcebase material: leaded free-machining brass CuZn39Pb2 (C37700), Wieland-Z30 rolled products, reference value at room temperature | 0.3sourcedesign value (structural stainless steels) |
| Shear modulus | 36GPa | 76.9GPa2.14x stiffer in shear |
| Bulk modulus | 101GPa | 167GPa |
| Speed of sound | 3,370m/s | 4,992m/s |
| Thermal | ||
| Thermal conductivity | 116W/m·Ksourcetypical, 20 °C | 14.6W/m·Ksource20–100 °C |
| Thermal expansion | 20.5µm/m·Ksourcetypical, mean 20-300 °C | 16.5µm/m·Ksourcemean, 20–100 °C |
| 100 mm part over a 50 °C swing | 103µm growth | 82.5µm growth24% less |
| Specific heat | 377J/kg·Ksourcetypical, 20 °C | 450J/kg·Ksourceat 20 °C |
| Heats up and cools (diffusivity) | 36.2mm²/s8.96x faster | 4.04mm²/s |
| Thermal shock resistance | 11,997W/m14.6x more resistant | 821W/m |
| Melting point | 888–899°Csourcesolidus-liquidus | 1,390–1,440°Csourcemelting range |
| Max service temperature | not sourced | 871–899°Csourceoxidation (scaling) limit in air |
| Values for | C36000 free-cutting brass, H02 half-hard rod 1 in. section (20% cold work), copper.org typical values | ATI 316 (UNS S31600), annealed 1.0 mm sheet, ATI technical data sheet (2012); Poisson's ratio from the Nickel Institute/SCI structural stainless design manual |
Every value links to the document that states it. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.
Questions
Is Brass C360 stronger than Stainless Steel 316?
Brass C360 is stronger: its yield strength is 310 MPa against 265 MPa for Stainless Steel 316 (17%).
Which is lighter, Brass C360 or Stainless Steel 316?
Stainless Steel 316 is lighter: 8,027 kg/m³ against 8,498 kg/m³ for Brass C360.
Which is stiffer, Brass C360 or Stainless Steel 316?
Stainless Steel 316 is stiffer: Young's modulus 200 GPa against 96.5 GPa for Brass C360, so the same part in Stainless Steel 316 deflects less under the same load.
Which is lighter for the same job, Brass C360 or Stainless Steel 316?
For the same stiffness or strength: Brass C360 is lighter for a strong rod or tie, strong beam, strong panel or plate; Stainless Steel 316 is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate.
| Part that must be | Brass C360 | Stainless Steel 316 |
|---|---|---|
| Stiff rod or tie (tension) | 2.19x heavier | lighter |
| Stiff beam (bending) | 1.52x heavier | lighter |
| Stiff panel or plate | 35% heavier | lighter |
| Strong rod or tie | lighter | 10% heavier |
| Strong beam | lighter | 5% heavier |
| Strong panel or plate | lighter | 2% heavier |
For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).
Which conducts heat better, Brass C360 or Stainless Steel 316?
Brass C360 conducts heat better: 116 W/m·K against 14.6 W/m·K for Stainless Steel 316.
Which expands less with temperature?
Stainless Steel 316 expands less: 16.5 µm/m·K against 20.5 µm/m·K for Brass C360.