Materials / Stainless Steel

Stainless Steel 316

Stainless Steel 316 (marine) strength, stiffness, density and thermal properties, with their source.

A bracket in Stainless Steel 316, brushed finish.

ProcessWrought
Mechanical
Yield strength265MPasourcetypical (representative), annealed 1.0 mm sheet
Ultimate tensile strength583MPasourcetypical (representative), annealed 1.0 mm sheet
Elongation at break61%sourcetypical (representative), annealed, in 2 in. (51 mm)
Young's modulus (stiffness)200GPasourcetypical, in tension
Density8,027kg/m³sourcetypical
Strength to weight33kN·m/kg
Stiffness to weight24.9MN·m/kg
Poisson's ratio0.3sourcedesign value (structural stainless steels)
Shear modulus76.9GPa
Bulk modulus167GPa
Speed of sound4,992m/s
Thermal
Thermal conductivity14.6W/m·Ksource20–100 °C
Thermal expansion16.5µm/m·Ksourcemean, 20–100 °C
100 mm part over a 50 °C swing82.5µm growth
Specific heat450J/kg·Ksourceat 20 °C
Heats up and cools (diffusivity)4.04mm²/s
Thermal shock resistance821W/m
Melting point1,390–1,440°Csourcemelting range
Max service temperature871–899°Csourceoxidation (scaling) limit in air
Values forATI 316 (UNS S31600), annealed 1.0 mm sheet, ATI technical data sheet (2012); Poisson's ratio from the Nickel Institute/SCI structural stainless design manual

Among 59 materials

1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelStainless Steel 316
Stiffness against density
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickStainless Steel 316
Strength against density

Compare Stainless Steel 316 with