Thermal conductivity against densityHigher and further left: spreads more heat for its weightThermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA sample part to run stress or thermal on, free in your browser
Sources7 documents: Outokumpu, National Institute of Standards and Technology, Brick Industry Association, Steel Construction Institute, Carpenter Technology
Brick
Solid extruded clay/shale brick units (BIA 1993 manufacturer survey, TN 3A 2024); face brick of 130 lb/ft3 for thermal properties (BIA TN 4, from ASHRAE 2013); CTE is the TMS Code value for clay/shale masonry
Stainless Steel 303
1.4305 / UNS S30300, Outokumpu typical values (hot rolled, solution annealed) from 'Steel Grades, Properties and Global Standards'; max service from Carpenter CarTech 303 datasheet
1
Steel Grades, Properties and Global StandardsOutokumpuarchived copyStainless Steel 303 · Yield strength: Outokumpu typical (product P = hot rolled plate, transverse)Stainless Steel 303 · Ultimate tensile strength: Outokumpu typicalStainless Steel 303 · Elongation at break: Outokumpu typical, A5Stainless Steel 303 · Young's modulus (stiffness): at RT (Table 12)Stainless Steel 303 · Density: at RTStainless Steel 303 · Thermal conductivity: at RTStainless Steel 303 · Thermal expansion: mean, 20–100 °CStainless Steel 303 · Specific heat: at RT
2
Strength of Masonry Walls Under Compressive and Transverse Loads (Building Science Series 34)National Institute of Standards and Technologyarchived copyBrick · Ultimate tensile strength: modulus of rupture (no direct tensile value)
3
Technical Notes 3A: Brick Masonry Material PropertiesBrick Industry AssociationBrick · Compressive strength: mean unit compressive strength, solid extruded brick (survey mean; SD 30.8 MPa)Brick · Thermal expansion: TMS Code average coefficient, clay/shale unit masonry
4
Technical Notes 4: Introduction to Energy Performance of Brick Masonry (2016)Brick Industry Associationarchived copyBrick · Density: face brick density row used for k (BIA notes most fired clay brick 120-130 lb/ft3)Brick · Thermal conductivity: range for 130 lb/ft3 face brick (ASHRAE 2013 via BIA)
5
Design Manual for Structural Stainless Steel, 4th Edition (P413)Steel Construction Institutearchived copyStainless Steel 303 · Poisson's ratio: design value (structural stainless steels)
6
Technical Notes 4B: Energy Code Compliance of Brick Masonry WallsBrick Industry Associationarchived copyBrick · Specific heat: value used in BIA heat-capacity sample calculation
7
Carpenter Stainless Type 303 Data SheetCarpenter Technologyarchived copyStainless Steel 303 · Max service temperature: continuous, scaling limit
Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.
Questions
Mechanical
Is Brick stronger than Stainless Steel 303?
Stainless Steel 303 is stronger: its yield strength is 275 MPa against tensile strength 5.1 MPa for Brick (53.9x).
Which is lighter, Brick or Stainless Steel 303?
Brick is lighter: 2,082 kg/m³ against 7,900 kg/m³ for Stainless Steel 303.
Which is lighter for the same job, Brick or Stainless Steel 303?
For the same stiffness or strength: Stainless Steel 303 is lighter for a strong rod or tie, strong beam, strong panel or plate.
Part that must be
Brick
Stainless Steel 303
Strong rod or tie
14.2x heavier
lighter
Strong beam
3.76x heavier
lighter
Strong panel or plate
1.94x heavier
lighter
For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).
Thermal
Which conducts heat better, Brick or Stainless Steel 303?
Stainless Steel 303 conducts heat better: 15 W/m·K against 1.02 W/m·K for Brick.
Which expands less with temperature?
Brick expands less: 7.2 µm/m·K against 16 µm/m·K for Stainless Steel 303.