Materials / Compare

Copper C12200 vs. Steel A992

Compare Copper C12200 vs. Steel A992 strength, stiffness, weight and thermal properties.

Copper C12200Wrought
Steel A992Wrought
MechanicalCopper C12200Steel A992
Yield strength69MPa1385MPa25.58x stronger
Ultimate tensile strength221MPa1505MPa22.29x stronger
Elongation at break45%11.86x more ductile24.2%2
Young's modulus (stiffness)117GPa1design value200GPa3
Density8,941kg/m³17,850kg/m³414% lighter
Strength to weight7.72kN·m/kg49kN·m/kg6.36x higher
Stiffness to weight13.1MN·m/kg25.5MN·m/kg1.94x higher
Poisson's ratio0.345design value0.33
Shear modulus43.7GPa76.9GPa1.76x stiffer in shear
Bulk modulus122GPa167GPa37% higher
Speed of sound3,621m/s5,048m/s39% faster
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100GlassSteel AISI 1045Steel AISI 4340Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Copper C12200Steel A992
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100GlassSteel AISI 1045Steel AISI 4340Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Copper C12200Steel A992
Strength against densityHigher and further left: stronger for its weight
ThermalCopper C12200Steel A992
Thermal conductivity339W/m·K17.07x more heat through a fin48W/m·K4
Thermal expansion16.9µm/m·K112µm/m·K441% less
100 mm part over a 50 °C swing84.5µm growth60µm growth41% less
Specific heat385J/kg·K1base material460–480J/kg·K6
Heats up and cools (diffusivity)98.5mm²/s7.57x faster13mm²/s
Thermal shock resistance7,799W/m45% more resistant5,390W/m
Melting pointliquidus1,083°C1not sourced
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100GlassSteel AISI 1045Steel AISI 4340Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Copper C12200Steel A992
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100GlassSteel AISI 1045Steel AISI 4340Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Copper C12200Steel A992
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources6 documents: Copper Development Association, American Institute of Steel Construction, bauforumstahl (ArcelorMittal), Wieland, Ovako
Copper C12200
C12200 phosphorus-deoxidized copper (DHP, the air-conditioning and refrigeration tube copper), tube annealed to 0.050 mm grain size (OS050), 0.065 in. wall, copper.org typical values
Steel A992
ASTM A992 W-shapes; Fy/Fu specified minimums from AISC publications (AISC 360-16 Commentary; Modern Steel Construction); elastic constants AISC 360; physical constants from the bauforumstahl structural-steel EPD, which names A992 among covered product standards.
  1. 1
    C12200 Alloy (copper.org)Copper Development Associationarchived copyCopper C12200 · Yield strength: typical, 0.5% extension under load, 0.065 in. tubeCopper C12200 · Ultimate tensile strength: typical, 0.065 in. tubeCopper C12200 · Elongation at break: typical, 0.065 in. tubeCopper C12200 · Young's modulus (stiffness): typicalCopper C12200 · Density: nominalCopper C12200 · Thermal conductivity: typical, 20 °CCopper C12200 · Thermal expansion: typical, mean 20-100 °CCopper C12200 · Specific heat: typical, 20 °CCopper C12200 · Melting point: liquidus
  2. 2
    Updating Standard Shape Material Properties Database for Design and ReliabilityAmerican Institute of Steel Constructionarchived copySteel A992 · Yield strength: typical: mean of 20,295 A992 flange mill-test coupons (1998 SSPC survey), as reported by AISCSteel A992 · Ultimate tensile strength: typical: mean of 20,295 A992 flange mill-test coupons (1998 SSPC survey)Steel A992 · Elongation at break: typical: mean of 24,847 A992 mill-test elongations, web and flange (1998 SSPC mill data), as reported by AISC
  3. 3
    ANSI/AISC 360-16 Specification for Structural Steel Buildings, with CommentaryAmerican Institute of Steel Constructionarchived copySteel A992 · Young's modulus (stiffness): design value (AISC 360-16)Steel A992 · Poisson's ratio: design value (AISC 360-16 Commentary)
  4. 4
    Environmental Product Declaration: Structural Steel Sections and Merchant Bars (2023)bauforumstahl (ArcelorMittal)archived copySteel A992 · Density: nominal (constructional data)Steel A992 · Thermal conductivity: nominal at 20 °CSteel A992 · Thermal expansion: nominal (constructional data, no temperature range stated)
  5. 5
    Wieland-K19 (Cu-DHP, C12200) Data SheetWielandarchived copyCopper C12200 · Poisson's ratio: reference value at room temperature (Wieland-K19 = Cu-DHP = C12200, rolled products)
  6. 6
    S275JR Steel GradeOvakoSteel A992 · Specific heat: base material: EN S275JR unalloyed structural steel (the EN counterpart of A36), typical, 50/100 °C

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Questions

Mechanical

Is Copper C12200 stronger than Steel A992?

Steel A992 is stronger: its yield strength is 385 MPa against 69 MPa for Copper C12200 (5.58x).

Which is lighter, Copper C12200 or Steel A992?

Steel A992 is lighter: 7,850 kg/m³ against 8,941 kg/m³ for Copper C12200.

Which is stiffer, Copper C12200 or Steel A992?

Steel A992 is stiffer: Young's modulus 200 GPa against 117 GPa for Copper C12200, so the same part in Steel A992 deflects less under the same load.

Which is lighter for the same job, Copper C12200 or Steel A992?

For the same stiffness or strength: Steel A992 is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.

Part that must beCopper C12200Steel A992
Stiff rod or tie (tension)1.94x heavierlighter
Stiff beam (bending)49% heavierlighter
Stiff panel or plate36% heavierlighter
Strong rod or tie6.36x heavierlighter
Strong beam3.58x heavierlighter
Strong panel or plate2.69x heavierlighter

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Copper C12200 or Steel A992?

Copper C12200 stretches further before it breaks: 45% elongation at break against 24.2% for Steel A992.

Thermal

Which conducts heat better, Copper C12200 or Steel A992?

Copper C12200 conducts heat better: 339 W/m·K against 48 W/m·K for Steel A992.

Which expands less with temperature?

Steel A992 expands less: 12 µm/m·K against 16.9 µm/m·K for Copper C12200.