Yield strength530MPa1not given (tensile used)
Ultimate tensile strength640MPa1modulus of rupture99MPa2
Compressive strengthnot sourced46.6MPa2
Flexural strengthnot sourcedmodulus of rupture99MPa2
Elongation at break40%1not sourced
Young's modulus (stiffness)185GPa314.8x stifferbending MOE12.5GPa2
Densitypart density7,900kg/m³4681–702kg/m³5
Strength to weight67.1kN·m/kg143kN·m/kg2.13x higher
Stiffness to weight23.4MN·m/kg30% higher18.1MN·m/kg
Poisson's ratiobase material0.36mu_LR0.352
Shear modulus71.2GPa15.4x stiffer in shear4.63GPa
Bulk modulus154GPa11.1x higher13.9GPa
Speed of sound4,839m/s14% faster4,252m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS 316L Stainless SteelWood
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS 316L Stainless SteelWood
Strength against densityHigher and further left: stronger for its weight
ThermalDMLS 316L Stainless SteelWood
Thermal conductivitybase material16.2W/m·K790x more heat through a finacross grain0.18W/m·K8
Thermal expansionmean 25-100 °C15.7µm/m·K1parallel to grain3.1–4.5µm/m·K8
100 mm part over a 50 °C swing78.6µm growth19µm growth4.14x less
Specific heatbase material500J/kg·K7solid wood1,700J/kg·K83.4x higher
Heats up and cools (diffusivity)4.1mm²/s26.8x faster0.153mm²/s
Thermal shock resistance2,067W/m8.47x more resistant244W/m
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS 316L Stainless SteelWood
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS 316L Stainless SteelWood
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources8 documents: EOS GmbH, USDA Forest Products Laboratory, Steel Construction Institute, Cleveland-Cliffs
DMLS 316L Stainless Steel
EOS StainlessSteel 316L (powder 9011-0032), EOS M 290, ParameterSet 316L 20µm Surface M290/400W, as manufactured, horizontal; ISO 6892-1
Wood
Northern red oak (Quercus rubra), clear straight-grained specimens at 12% MC, parallel to grain unless stated; USDA FPL Wood Handbook FPL-GTR-282 (2021) Ch. 4 and Ch. 5
  1. 1
    EOS StainlessSteel 316L Material Data SheetEOS GmbHarchived copyDMLS 316L Stainless Steel · Yield strength: typical, as manufactured, horizontalDMLS 316L Stainless Steel · Ultimate tensile strength: typical, as manufactured, horizontalDMLS 316L Stainless Steel · Elongation at break: typical at break, as manufactured, horizontalDMLS 316L Stainless Steel · Thermal expansion: mean 25-100 °C, ASTM E228
  2. 2
    Wood Handbook (FPL-GTR-282), Chapter 5: Mechanical Properties of WoodUSDA Forest Products LaboratoryWood · Ultimate tensile strength: modulus of rupture (no direct tensile value)Wood · Compressive strength: compression parallel to grain (maximum crushing strength), 12% MCWood · Flexural strength: modulus of rupture (static bending), 12% MCWood · Young's modulus (stiffness): bending MOE, parallel to grainWood · Poisson's ratio: mu_LR (red oak group, ~12% MC)
  3. 3
    EOS StainlessSteel 316L Material Data Sheet, M 280 and M 290 (2014)EOS GmbHarchived copyDMLS 316L Stainless Steel · Young's modulus (stiffness): typical, as built, horizontal (XY); EOSINT M280-400W / M290-400W, 316L_Surface 1.0, 20 µm (2014 sheet)
  4. 4
    EOS StainlessSteel 316L Material Data Sheet, FlexLine, M 290 (2016)EOS GmbHarchived copyDMLS 316L Stainless Steel · Density: part density (ISO 3369, not labelled min or typical), EOS M 290, 40 µm FlexLine
  5. 5
    Technical Note 218: Weights of Various Woods Grown in the United States (1953)USDA Forest Products LaboratoryWood · Density: average weight of clear wood at 8% and 15% moisture content
  6. 6
    Design Manual for Structural Stainless Steel, 4th Edition (P413)Steel Construction Institutearchived copyDMLS 316L Stainless Steel · Poisson's ratio: base material: austenitic stainless steels incl. 1.4404 (316L), design value
  7. 7
    316/316L Stainless Steel Product Data Bulletin (2021)Cleveland-CliffsDMLS 316L Stainless Steel · Thermal conductivity: base material: wrought 316/316L (Cleveland-Cliffs), at 100 °CDMLS 316L Stainless Steel · Specific heat: base material: wrought 316/316L (Cleveland-Cliffs), 0-100 °C
  8. 8
    Wood Handbook (FPL-GTR-282), Chapter 4: Moisture Relations and Physical Properties of WoodUSDA Forest Products LaboratoryWood · Thermal conductivity: across grain, 12% MC (Table 4-7, approximate)Wood · Thermal expansion: parallel to grain, ovendry wood, range across speciesWood · Specific heat: solid wood (all species), 12% MC, 27 C

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

DMLS 316L Stainless Steel is 3D printed: its properties depend on build direction and print settings; these are typical values.

Questions

Mechanical

Is DMLS 316L Stainless Steel stronger than Wood?

DMLS 316L Stainless Steel is stronger: its yield strength is 530 MPa against tensile strength 99 MPa for Wood (5.35x).

Which is lighter, DMLS 316L Stainless Steel or Wood?

Wood is lighter: 692 kg/m³ against 7,900 kg/m³ for DMLS 316L Stainless Steel.

Which is stiffer, DMLS 316L Stainless Steel or Wood?

DMLS 316L Stainless Steel is stiffer: Young's modulus 185 GPa against 12.5 GPa for Wood, so the same part in DMLS 316L Stainless Steel deflects less under the same load.

Which is lighter for the same job, DMLS 316L Stainless Steel or Wood?

For the same stiffness or strength: DMLS 316L Stainless Steel is lighter for a stiff rod or tie (tension); Wood is lighter for a stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.

Part that must beDMLS 316L Stainless SteelWood
Stiff rod or tie (tension)lighter30% heavier
Stiff beam (bending)2.97x heavierlighter
Stiff panel or plate4.65x heavierlighter
Strong rod or tie2.13x heavierlighter
Strong beam3.73x heavierlighter
Strong panel or plate4.94x heavierlighter

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Thermal

Which conducts heat better, DMLS 316L Stainless Steel or Wood?

DMLS 316L Stainless Steel conducts heat better: 16.2 W/m·K against 0.18 W/m·K for Wood.

Which expands less with temperature?

Wood expands less: 3.8 µm/m·K against 15.7 µm/m·K for DMLS 316L Stainless Steel.

Related comparisons