Materials / DMLS

DMLS 316L Stainless Steel

DMLS 316L Stainless Steel strength, stiffness, density and thermal properties, with their source.

A bracket in DMLS 316L Stainless Steel, as-sintered finish.

Process3D printed metal (DMLS)
Mechanical
Yield strength530MPasourcetypical, as manufactured, horizontal
Ultimate tensile strength640MPasourcetypical, as manufactured, horizontal
Elongation at break40%sourcetypical at break, as manufactured, horizontal
Young's modulus (stiffness)185GPasourcetypical, as built, horizontal (XY); EOSINT M280-400W / M290-400W, 316L_Surface 1.0, 20 µm (2014 sheet)
Density7,900kg/m³sourcepart density (ISO 3369, not labelled min or typical), EOS M 290, 40 µm FlexLine
Strength to weight67.1kN·m/kg
Stiffness to weight23.4MN·m/kg
Poisson's ratio0.3sourcebase material: austenitic stainless steels incl. 1.4404 (316L), design value
Shear modulus71.2GPa
Bulk modulus154GPa
Speed of sound4,839m/s
Thermal
Thermal conductivity16.2W/m·Ksourcebase material: wrought 316/316L (Cleveland-Cliffs), at 100 °C
Thermal expansion15.7µm/m·Ksourcemean 25-100 °C, ASTM E228
100 mm part over a 50 °C swing78.6µm growth
Specific heat500J/kg·Ksourcebase material: wrought 316/316L (Cleveland-Cliffs), 0-100 °C
Heats up and cools (diffusivity)4.1mm²/s
Thermal shock resistance2,067W/m
Values forEOS StainlessSteel 316L (powder 9011-0032), EOS M 290, ParameterSet 316L 20µm Surface M290/400W, as manufactured, horizontal; ISO 6892-1

DMLS 316L Stainless Steel is 3D printed: its properties depend on build direction and print settings; these are typical values.

Among 59 materials

1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 17-4PH Stainless SteelDMLS 316L Stainless Steel
Stiffness against density
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 17-4PH Stainless SteelBrickDMLS 316L Stainless Steel
Strength against density

Compare DMLS 316L Stainless Steel with