Materials / Compare
Drywall vs. Plastic TPU Compare Drywall vs. Plastic TPU strength, stiffness, weight and thermal properties.
Change either side
Plastic PLA Plastic PETG Plastic ABS Plastic TPU Plastic Nylon Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic POM/Acetal Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic PTFE Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA Rubber Wood Aluminum Aluminum 6061-T6 Aluminum 7075-T6 Aluminum 2024-T351 Aluminum 5052-H32 Aluminum 7050-T7451 Steel Steel AISI 1018 Steel AISI 1045 Steel AISI 4340 Steel A992 Iron Titanium Titanium Ti-6Al-4V Stainless 304 Stainless 316 Stainless 303 Stainless 17-4PH Brass C360 Brass C260 Copper C110 Glass Nickel Inconel 718 Magnesium AZ31B-H24 Zinc Zamak 3 FDM ASA FDM Polycarbonate FDM PAHT-CF FDM HIPS SLA Resin Standard SLA Resin Tough 2000 SLA Resin Elastic 50A SLS PA12 Nylon DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel Concrete Brick Plywood Drywall Drywall Natural Plastic PLA Plastic PETG Plastic ABS Plastic TPU Plastic Nylon Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic POM/Acetal Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic PTFE Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA Rubber Wood Aluminum Aluminum 6061-T6 Aluminum 7075-T6 Aluminum 2024-T351 Aluminum 5052-H32 Aluminum 7050-T7451 Steel Steel AISI 1018 Steel AISI 1045 Steel AISI 4340 Steel A992 Iron Titanium Titanium Ti-6Al-4V Stainless 304 Stainless 316 Stainless 303 Stainless 17-4PH Brass C360 Brass C260 Copper C110 Glass Nickel Inconel 718 Magnesium AZ31B-H24 Zinc Zamak 3 FDM ASA FDM Polycarbonate FDM PAHT-CF FDM HIPS SLA Resin Standard SLA Resin Tough 2000 SLA Resin Elastic 50A SLS PA12 Nylon DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel Concrete Brick Plywood Drywall Plastic TPU 3D printed (FDM) Try it on a partA sample part to run stress or thermal on, free in your browser Open in LessCAD Open in LessCAD Mechanical Yield strength not given (tensile used) not given (tensile used) Ultimate tensile strength 1–2 MPa source ambient range reported in review (Australian studies) 23.7 MPa source typical, stress at break Compressive strength 2.4 MPa source typical, 70 F / 50% RH not sourced Flexural strength not sourced 4.1 MPa source typical Elongation at break not sourced not sourced Young's modulus (stiffness) 1–2 GPa source ambient range reported in review (Australian studies) 0.067 GPa source typical Density not sourced 1,220 kg/m³ source typical Strength to weight not sourced 19.4 kN·m/kg Stiffness to weight not sourced 0.0549 MN·m/kg Poisson's ratio not sourced not sourced Shear modulus not sourced not sourced Bulk modulus not sourced not sourced Speed of sound not sourced 234 m/s Thermal Thermal conductivity not sourced not sourced Thermal expansion 16.7 µm/m·K source typical, unrestrained, 3.3-32 C not sourced 100 mm part over a 50 °C swing 83.5 µm growth not sourced Specific heat 1,090 J/kg·K source typical (from ASHRAE Handbook of Fundamentals, per GA) not sourced Heats up and cools (diffusivity) not sourced not sourced Thermal shock resistance not sourced not sourced Melting point not sourced 217 °C source typical Max service temperature 52 °C source manufacturer sustained-exposure limit 50.3 °C source HDT 0.455 MPa (printed specimens) Values for 1/2 in. (12.7 mm) regular gypsum board (ASTM C1396), Gypsum Association GA-235-2019 typical/minimum properties; tensile and E from USDA FPL-co-authored review; service limit from USG Sheetrock 1/2 in. submittal Ultimaker TPU 95A, 3D-printed specimens, XY (flat); Ultimaker S5 Pro, engineering intent profile, 0.15 mm layer height, AA 0.4 print core, 100% infill, Cura 4.9, printed one-at-a-time, conditioned >=24 h at room temperature. TDS (file v5.00), April 29, 2022.
Every value links to the document that states it. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.
Plastic TPU is 3D printed: its properties depend on build direction and print settings; these are typical values.
Questions Is Drywall stronger than Plastic TPU? Plastic TPU is stronger: its tensile strength is 23.7 MPa against 1.5 MPa for Drywall (15.8x).
Which is stiffer, Drywall or Plastic TPU? Drywall is stiffer: Young's modulus 1.5 GPa against 0.067 GPa for Plastic TPU, so the same part in Drywall deflects less under the same load.
Among 59 materials 1k 10k 0.1 1 10 100 Density (kg/m³) Young's modulus (GPa) Plastic PLA Plastic PETG Plastic ABS Plastic Nylon Aluminum Steel Iron Titanium Steel AISI 1018 Stainless 304 Stainless 316 Aluminum 6061-T6 Aluminum 7075-T6 Brass C360 Copper C110 Glass Steel AISI 1045 Steel AISI 4340 Steel A992 Stainless 303 Stainless 17-4PH Aluminum 2024-T351 Aluminum 5052-H32 Aluminum 7050-T7451 Titanium Ti-6Al-4V Brass C260 Nickel Inconel 718 Magnesium AZ31B-H24 Zinc Zamak 3 Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic POM/Acetal Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA FDM ASA FDM Polycarbonate FDM PAHT-CF FDM HIPS SLA Resin Tough 2000 SLS PA12 Nylon DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel Plastic TPU Stiffness against density 1k 10k 10 100 1k Density (kg/m³) Yield strength (MPa) Plastic PLA Plastic PETG Plastic ABS Plastic Nylon Rubber Aluminum Steel Iron Titanium Steel AISI 1018 Stainless 304 Stainless 316 Aluminum 6061-T6 Aluminum 7075-T6 Brass C360 Copper C110 Glass Steel AISI 1045 Steel AISI 4340 Steel A992 Stainless 303 Stainless 17-4PH Aluminum 2024-T351 Aluminum 5052-H32 Aluminum 7050-T7451 Titanium Ti-6Al-4V Brass C260 Nickel Inconel 718 Magnesium AZ31B-H24 Zinc Zamak 3 Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic POM/Acetal Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic PTFE Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA FDM ASA FDM Polycarbonate FDM PAHT-CF FDM HIPS SLA Resin Tough 2000 SLA Resin Elastic 50A SLS PA12 Nylon DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel Brick Plastic TPU Strength against density