Materials / Compare

FDM PAHT-CF vs. Plastic Polycarbonate

Compare FDM PAHT-CF vs. Plastic Polycarbonate strength, stiffness, weight and thermal properties.

Change either side
FDM PAHT-CF3D printed (FDM)
Plastic PolycarbonateBulk polymer (molded or machined)
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Mechanical
Yield strengthnot given (tensile used)65MPasourcetypical, tensile yield
Ultimate tensile strength92MPasourcetypical65MPasourcetypical, stress at break
Flexural strength125MPasourcetypical97MPasourcetypical, flexural strength
Elongation at break8.4%sourcetypical125%sourcetypical, strain at break
Young's modulus (stiffness)3.86GPasourcetypical1.61x stiffer2.4GPasourcetypical
Density1,060kg/m³sourcetypical13% lighter1,200kg/m³sourcetypical
Strength to weight86.8kN·m/kg1.6x higher54.2kN·m/kg
Stiffness to weight3.64MN·m/kg1.82x higher2MN·m/kg
Poisson's rationot sourced0.38sourcetypical, polycarbonate family (Covestro Part and Mold Design guide, Table 3-1)
Shear modulusnot sourced0.87GPa
Bulk modulusnot sourced3.33GPa
Speed of sound1,908m/s1,414m/s
Thermal
Thermal conductivitynot sourced0.2W/m·Ksourcetypical, through-plane, 23 C
Thermal expansionnot sourced65µm/m·Ksourcetypical, 23-55 C, parallel and normal
100 mm part over a 50 °C swingnot sourced325µm growth
Specific heatnot sourced1,172J/kg·Ksourcetypical (guide value), Bayer ASTM datasheet for Makrolon 2405, ASTM D 2766
Heats up and cools (diffusivity)not sourced0.142mm²/s
Thermal shock resistancenot sourced51.7W/m
Melting point225°Csourcetypicalnot sourced
Glass transition70°Csourcetypical144°Csourcetypical, DSC 10 C/min
Max service temperature170°CsourceHDT 1.8 MPa125°CsourceUL 746B RTI, tensile strength, 1.5 mm
Values forBambu Lab PAHT-CF, TDS V3.0, printed specimens X-Y, dry state; nozzle 290 °C, bed 100 °C, 100 mm/s, 100% infill; annealed and dried 80 °C for 12 h before testing.Covestro Makrolon 2405 general-purpose PC (MVR 19), Covestro technical datasheet version 2026-09-28, typical values

Every value links to the document that states it. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

FDM PAHT-CF is 3D printed: its properties depend on build direction and print settings; these are typical values.

Questions

Is FDM PAHT-CF stronger than Plastic Polycarbonate?

FDM PAHT-CF is stronger: its tensile strength is 92 MPa against yield strength 65 MPa for Plastic Polycarbonate (42%).

Which is lighter, FDM PAHT-CF or Plastic Polycarbonate?

FDM PAHT-CF is lighter: 1,060 kg/m³ against 1,200 kg/m³ for Plastic Polycarbonate.

Which is stiffer, FDM PAHT-CF or Plastic Polycarbonate?

FDM PAHT-CF is stiffer: Young's modulus 3.86 GPa against 2.4 GPa for Plastic Polycarbonate, so the same part in FDM PAHT-CF deflects less under the same load.

Which is lighter for the same job, FDM PAHT-CF or Plastic Polycarbonate?

For the same stiffness or strength: FDM PAHT-CF is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.

Part that must beFDM PAHT-CFPlastic Polycarbonate
Stiff rod or tie (tension)lighter1.82x heavier
Stiff beam (bending)lighter44% heavier
Stiff panel or platelighter33% heavier
Strong rod or tielighter1.6x heavier
Strong beamlighter43% heavier
Strong panel or platelighter35% heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Among 59 materials

1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelFDM PAHT-CFPlastic Polycarbonate
Stiffness against density
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickFDM PAHT-CFPlastic Polycarbonate
Strength against density

Related comparisons