Magnesium AZ31B-H24 vs. Magnesium AZ91D Compare Magnesium AZ31B-H24 vs. Magnesium AZ91D strength, stiffness, weight and thermal properties.
Change either side
Plastic PLA Plastic PETG Plastic ABS Plastic TPU Plastic Nylon Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic POM/Acetal Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic PTFE Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA Plastic PBT GF30 Plastic PPS GF40 Plastic LCP GF30 Rubber Wood Aluminum Aluminum 6061-T6 Aluminum 7075-T6 Aluminum 2024-T351 Aluminum 5052-H32 Aluminum 7050-T7451 Aluminum A380 Aluminum 6063-T6 Aluminum 1100-O Aluminum ADC12 Steel Steel AISI 1018 Steel AISI 1045 Steel AISI 4340 Steel A992 Iron Titanium Titanium Ti-6Al-4V Stainless Steel 304 Stainless Steel 316 Stainless Steel 303 Stainless Steel 17-4PH Brass C360 Brass C260 Copper C110 Glass Nickel Inconel 718 Magnesium AZ31B-H24 Magnesium AZ91D Zinc Zamak 3 FDM ASA FDM Polycarbonate FDM PAHT-CF FDM HIPS SLA Resin Standard SLA Resin Tough 2000 SLA Resin Elastic 50A SLS PA12 Nylon DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel Concrete Brick Plywood Drywall PCB Laminate FR-4 Silicon Ceramic Alumina 96% Ceramic Aluminum Nitride Solder SAC305 Magnesium AZ31B-H24 Wrought Plastic PLA Plastic PETG Plastic ABS Plastic TPU Plastic Nylon Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic POM/Acetal Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic PTFE Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA Plastic PBT GF30 Plastic PPS GF40 Plastic LCP GF30 Rubber Wood Aluminum Aluminum 6061-T6 Aluminum 7075-T6 Aluminum 2024-T351 Aluminum 5052-H32 Aluminum 7050-T7451 Aluminum A380 Aluminum 6063-T6 Aluminum 1100-O Aluminum ADC12 Steel Steel AISI 1018 Steel AISI 1045 Steel AISI 4340 Steel A992 Iron Titanium Titanium Ti-6Al-4V Stainless Steel 304 Stainless Steel 316 Stainless Steel 303 Stainless Steel 17-4PH Brass C360 Brass C260 Copper C110 Glass Nickel Inconel 718 Magnesium AZ31B-H24 Magnesium AZ91D Zinc Zamak 3 FDM ASA FDM Polycarbonate FDM PAHT-CF FDM HIPS SLA Resin Standard SLA Resin Tough 2000 SLA Resin Elastic 50A SLS PA12 Nylon DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel Concrete Brick Plywood Drywall PCB Laminate FR-4 Silicon Ceramic Alumina 96% Ceramic Aluminum Nitride Solder SAC305 Magnesium AZ91D Cast Try it on a partA bracket to run stress or thermal on, free in your browser Open in LessCAD Open in LessCAD Mechanical Yield strength 220 MPa source typical, H24, 0.5-6 mm, 0.2 % proof stress 150 MPa source typical, 0.2% tensile yield, ambient temperature Ultimate tensile strength 290 MPa source typical, H24, 0.5-6 mm 230 MPa source typical, ambient temperature Elongation at break 13 % source typical, H24, 0.5-6 mm, gauge 5.65√A 3 % source typical, ambient temperature Young's modulus (stiffness) 44.8 GPa source typical (handbook physical constant) 45 GPa source typical Density 1,769 kg/m³ source nominal 1,810 kg/m³ source typical Strength to weight 124 kN·m/kg 1.5x higher 82.9 kN·m/kg Stiffness to weight 25.3 MN·m/kg 2% higher 24.9 MN·m/kg Poisson's ratio 0.35 source typical (handbook physical constant) 0.35 source base material: AZ91C casting (MIL-HDBK-5J handbook physical constant) Shear modulus 16.6 GPa 16.7 GPa Bulk modulus 49.8 GPa 50 GPa Speed of sound 5,032 m/s 4,986 m/s Thermal Thermal conductivity 76.9 W/m·K source typical (temper/temperature not stated) 72 W/m·K source typical Thermal expansion 26.8 µm/m·K source typical (temperature range not stated) 25 µm/m·K source typical, temperature range not stated 100 mm part over a 50 °C swing 134 µm growth 125 µm growth 7% less Specific heat 1,040 J/kg·K source typical 1,050 J/kg·K source typical Heats up and cools (diffusivity) 41.8 mm²/s 10% faster 37.9 mm²/s Thermal shock resistance 9,159 W/m 47% more resistant 6,240 W/m Melting point not sourced 470–595 °C source melting range Max service temperature 149 °C source stated application limit not sourced Values for AZ31B-H24 sheet 0.016-0.062 in., MIL-HDBK-5J Table 4.2.1.0(b) (AMS 4377); strengths are S-basis MINIMUMS ELEKTRON AZ91D magnesium die-casting alloy, as cast; Magnesium Elektron datasheet 475 (7/01), typical properties; Poisson from MIL-HDBK-5J for AZ91C castings.
Every value links to the document that states it. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.
Questions Is Magnesium AZ31B-H24 stronger than Magnesium AZ91D? Magnesium AZ31B-H24 is stronger: its yield strength is 220 MPa against 150 MPa for Magnesium AZ91D (47%).
Which is lighter, Magnesium AZ31B-H24 or Magnesium AZ91D? Magnesium AZ31B-H24 is lighter: 1,769 kg/m³ against 1,810 kg/m³ for Magnesium AZ91D.
Which is stiffer, Magnesium AZ31B-H24 or Magnesium AZ91D? Magnesium AZ91D is stiffer: Young's modulus 45 GPa against 44.8 GPa for Magnesium AZ31B-H24, so the same part in Magnesium AZ91D deflects less under the same load.
Which is lighter for the same job, Magnesium AZ31B-H24 or Magnesium AZ91D? For the same stiffness or strength: Magnesium AZ31B-H24 is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.
Part that must be Magnesium AZ31B-H24 Magnesium AZ91D Stiff rod or tie (tension) lighter 2% heavier Stiff beam (bending) lighter 2% heavier Stiff panel or plate lighter 2% heavier Strong rod or tie lighter 1.5x heavier Strong beam lighter 32% heavier Strong panel or plate lighter 24% heavier
For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).
Which conducts heat better, Magnesium AZ31B-H24 or Magnesium AZ91D? Magnesium AZ31B-H24 conducts heat better: 76.9 W/m·K against 72 W/m·K for Magnesium AZ91D.
Which expands less with temperature? Magnesium AZ91D expands less: 25 µm/m·K against 26.8 µm/m·K for Magnesium AZ31B-H24.
Among 72 materials 1k 10k 0.1 1 10 100 Density (kg/m³) Young's modulus (GPa) Plastic PLA Plastic PETG Plastic ABS Plastic TPU Plastic Nylon Aluminum Steel Iron Titanium Steel AISI 1018 Stainless Steel 304 Stainless Steel 316 Aluminum 6061-T6 Aluminum 7075-T6 Brass C360 Copper C110 Glass Steel AISI 1045 Steel AISI 4340 Steel A992 Stainless Steel 303 Stainless Steel 17-4PH Aluminum 2024-T351 Aluminum 5052-H32 Aluminum 7050-T7451 Titanium Ti-6Al-4V Brass C260 Nickel Inconel 718 Zinc Zamak 3 Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic POM/Acetal Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA FDM ASA FDM Polycarbonate FDM PAHT-CF FDM HIPS SLA Resin Tough 2000 SLS PA12 Nylon DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel PCB Laminate FR-4 Silicon Ceramic Alumina 96% Ceramic Aluminum Nitride Aluminum A380 Aluminum 6063-T6 Aluminum 1100-O Aluminum ADC12 Solder SAC305 Plastic PBT GF30 Plastic PPS GF40 Plastic LCP GF30 Magnesium AZ31B-H24 Magnesium AZ91D Stiffness against density 1k 10k 10 100 1k Density (kg/m³) Yield strength (MPa) Plastic PLA Plastic PETG Plastic ABS Plastic TPU Plastic Nylon Rubber Aluminum Steel Iron Titanium Steel AISI 1018 Stainless Steel 304 Stainless Steel 316 Aluminum 6061-T6 Aluminum 7075-T6 Brass C360 Copper C110 Glass Steel AISI 1045 Steel AISI 4340 Steel A992 Stainless Steel 303 Stainless Steel 17-4PH Aluminum 2024-T351 Aluminum 5052-H32 Aluminum 7050-T7451 Titanium Ti-6Al-4V Brass C260 Nickel Inconel 718 Zinc Zamak 3 Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic POM/Acetal Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic PTFE Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA FDM ASA FDM Polycarbonate FDM PAHT-CF FDM HIPS SLA Resin Tough 2000 SLA Resin Elastic 50A SLS PA12 Nylon DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel Brick PCB Laminate FR-4 Silicon Ceramic Alumina 96% Aluminum A380 Aluminum 6063-T6 Aluminum 1100-O Aluminum ADC12 Solder SAC305 Plastic PBT GF30 Plastic PPS GF40 Plastic LCP GF30 Magnesium AZ31B-H24 Magnesium AZ91D Strength against density