Materials / Magnesium
Magnesium AZ31B-H24
Magnesium AZ31B-H24 strength, stiffness, density and thermal properties, with their source.
A bracket in Magnesium AZ31B-H24, brushed finish.
| Process | Wrought |
|---|
| Mechanical |
|---|
| Yield strength | 220MPasourcetypical, H24, 0.5-6 mm, 0.2 % proof stress |
|---|
| Ultimate tensile strength | 290MPasourcetypical, H24, 0.5-6 mm |
|---|
| Elongation at break | 13%sourcetypical, H24, 0.5-6 mm, gauge 5.65√A |
|---|
| Young's modulus (stiffness) | 44.8GPasourcetypical (handbook physical constant) |
|---|
| Density | 1,769kg/m³sourcenominal |
|---|
| Strength to weight | 124kN·m/kg |
|---|
| Stiffness to weight | 25.3MN·m/kg |
|---|
| Poisson's ratio | 0.35sourcetypical (handbook physical constant) |
|---|
| Shear modulus | 16.6GPa |
|---|
| Bulk modulus | 49.8GPa |
|---|
| Speed of sound | 5,032m/s |
|---|
| Thermal |
|---|
| Thermal conductivity | 76.9W/m·Ksourcetypical (temper/temperature not stated) |
|---|
| Thermal expansion | 26.8µm/m·Ksourcetypical (temperature range not stated) |
|---|
| 100 mm part over a 50 °C swing | 134µm growth |
|---|
| Specific heat | 1,040J/kg·Ksourcetypical |
|---|
| Heats up and cools (diffusivity) | 41.8mm²/s |
|---|
| Thermal shock resistance | 9,159W/m |
|---|
| Max service temperature | 149°Csourcestated application limit |
|---|
| Values for | AZ31B-H24 sheet 0.016-0.062 in., MIL-HDBK-5J Table 4.2.1.0(b) (AMS 4377); strengths are S-basis MINIMUMS |
|---|
Among 72 materials
Stiffness against densityStrength against density
Compare Magnesium AZ31B-H24 with