Plastic PLA Plastic PETG Plastic ABS Plastic TPU Plastic Nylon Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic POM/Acetal Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic PTFE Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA Plastic PBT GF30 Plastic PPS GF40 Plastic LCP GF30 Rubber Wood Aluminum Aluminum 6061-T6 Aluminum 7075-T6 Aluminum 2024-T351 Aluminum 5052-H32 Aluminum 7050-T7451 Aluminum A380 Aluminum 6063-T6 Aluminum 1100-O Aluminum ADC12 Steel Steel AISI 1018 Steel AISI 1045 Steel AISI 4340 Steel A992 Iron Titanium Titanium Ti-6Al-4V Stainless Steel 304 Stainless Steel 316 Stainless Steel 303 Stainless Steel 17-4PH Brass C360 Brass C260 Copper C110 Glass Nickel Inconel 718 Magnesium AZ31B-H24 Magnesium AZ91D Zinc Zamak 3 FDM ASA FDM Polycarbonate FDM PAHT-CF FDM HIPS SLA Resin Standard SLA Resin Tough 2000 SLA Resin Elastic 50A SLS PA12 Nylon DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel Concrete Brick Plywood Drywall PCB Laminate FR-4 Silicon Ceramic Alumina 96% Ceramic Aluminum Nitride Solder SAC305 Aluminum 2024-T351 Wrought Plastic PLA Plastic PETG Plastic ABS Plastic TPU Plastic Nylon Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic POM/Acetal Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic PTFE Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA Plastic PBT GF30 Plastic PPS GF40 Plastic LCP GF30 Rubber Wood Aluminum Aluminum 6061-T6 Aluminum 7075-T6 Aluminum 2024-T351 Aluminum 5052-H32 Aluminum 7050-T7451 Aluminum A380 Aluminum 6063-T6 Aluminum 1100-O Aluminum ADC12 Steel Steel AISI 1018 Steel AISI 1045 Steel AISI 4340 Steel A992 Iron Titanium Titanium Ti-6Al-4V Stainless Steel 304 Stainless Steel 316 Stainless Steel 303 Stainless Steel 17-4PH Brass C360 Brass C260 Copper C110 Glass Nickel Inconel 718 Magnesium AZ31B-H24 Magnesium AZ91D Zinc Zamak 3 FDM ASA FDM Polycarbonate FDM PAHT-CF FDM HIPS SLA Resin Standard SLA Resin Tough 2000 SLA Resin Elastic 50A SLS PA12 Nylon DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel Concrete Brick Plywood Drywall PCB Laminate FR-4 Silicon Ceramic Alumina 96% Ceramic Aluminum Nitride Solder SAC305 Magnesium AZ31B-H24 Wrought Try it on a partA bracket to run stress or thermal on, free in your browser Open in LessCAD Open in LessCAD Mechanical Yield strength 324 MPa source typical, 0.2% offset, .500 in dia specimen 220 MPa source typical, H24, 0.5-6 mm, 0.2 % proof stress Ultimate tensile strength 469 MPa source typical 290 MPa source typical, H24, 0.5-6 mm Elongation at break 19 % source typical, in 4D 13 % source typical, H24, 0.5-6 mm, gauge 5.65√A Young's modulus (stiffness) 73.1 GPa source typical 44.8 GPa source typical (handbook physical constant) Density 2,770 kg/m³ source nominal 1,769 kg/m³ source nominal 1.57x lighter Strength to weight 117 kN·m/kg 124 kN·m/kg 6% higher Stiffness to weight 26.4 MN·m/kg 4% higher 25.3 MN·m/kg Poisson's ratio 0.33 source typical (handbook physical constant), all tempers 0.35 source typical (handbook physical constant) Shear modulus 27.5 GPa 1.66x stiffer in shear 16.6 GPa Bulk modulus 71.7 GPa 49.8 GPa Speed of sound 5,137 m/s 5,032 m/s Thermal Thermal conductivity 120 W/m·K source typical, 20 °C 76.9 W/m·K source typical (temper/temperature not stated) Thermal expansion 22.9 µm/m·K source typical, mean 20-100 °C 26.8 µm/m·K source typical (temperature range not stated) 100 mm part over a 50 °C swing 115 µm growth 17% less 134 µm growth Specific heat 875 J/kg·K source typical, at 100 °C 1,040 J/kg·K source typical Heats up and cools (diffusivity) 49.5 mm²/s 18% faster 41.8 mm²/s Thermal shock resistance 15,561 W/m 1.7x more resistant 9,159 W/m Melting point 502–638 °C source melting range not sourced Max service temperature not sourced 149 °C source stated application limit Values for 2024-T4/T351, Kaiser Aluminum sheet, coil & plate typical datasheet; Poisson from MIL-HDBK-5J AZ31B-H24 sheet 0.016-0.062 in., MIL-HDBK-5J Table 4.2.1.0(b) (AMS 4377); strengths are S-basis MINIMUMS
Every value links to the document that states it. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.
Questions Is Aluminum 2024-T351 stronger than Magnesium AZ31B-H24? Aluminum 2024-T351 is stronger: its yield strength is 324 MPa against 220 MPa for Magnesium AZ31B-H24 (47%).
Which is lighter, Aluminum 2024-T351 or Magnesium AZ31B-H24? Magnesium AZ31B-H24 is lighter: 1,769 kg/m³ against 2,770 kg/m³ for Aluminum 2024-T351.
Which is stiffer, Aluminum 2024-T351 or Magnesium AZ31B-H24? Aluminum 2024-T351 is stiffer: Young's modulus 73.1 GPa against 44.8 GPa for Magnesium AZ31B-H24, so the same part in Aluminum 2024-T351 deflects less under the same load.
Which is lighter for the same job, Aluminum 2024-T351 or Magnesium AZ31B-H24? For the same stiffness or strength: Aluminum 2024-T351 is lighter for a stiff rod or tie (tension); Magnesium AZ31B-H24 is lighter for a stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.
Part that must be Aluminum 2024-T351 Magnesium AZ31B-H24 Stiff rod or tie (tension) lighter 4% heavier Stiff beam (bending) 23% heavier lighter Stiff panel or plate 33% heavier lighter Strong rod or tie 6% heavier lighter Strong beam 21% heavier lighter Strong panel or plate 29% heavier lighter
For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).
Which conducts heat better, Aluminum 2024-T351 or Magnesium AZ31B-H24? Aluminum 2024-T351 conducts heat better: 120 W/m·K against 76.9 W/m·K for Magnesium AZ31B-H24.
Which expands less with temperature? Aluminum 2024-T351 expands less: 22.9 µm/m·K against 26.8 µm/m·K for Magnesium AZ31B-H24.
Among 72 materials 1k 10k 0.1 1 10 100 Density (kg/m³) Young's modulus (GPa) Plastic PLA Plastic PETG Plastic ABS Plastic TPU Plastic Nylon Aluminum Steel Iron Titanium Steel AISI 1018 Stainless Steel 304 Stainless Steel 316 Aluminum 6061-T6 Aluminum 7075-T6 Brass C360 Copper C110 Glass Steel AISI 1045 Steel AISI 4340 Steel A992 Stainless Steel 303 Stainless Steel 17-4PH Aluminum 5052-H32 Aluminum 7050-T7451 Titanium Ti-6Al-4V Brass C260 Nickel Inconel 718 Zinc Zamak 3 Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic POM/Acetal Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA FDM ASA FDM Polycarbonate FDM PAHT-CF FDM HIPS SLA Resin Tough 2000 SLS PA12 Nylon DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel PCB Laminate FR-4 Silicon Ceramic Alumina 96% Ceramic Aluminum Nitride Aluminum A380 Aluminum 6063-T6 Aluminum 1100-O Aluminum ADC12 Magnesium AZ91D Solder SAC305 Plastic PBT GF30 Plastic PPS GF40 Plastic LCP GF30 Aluminum 2024-T351 Magnesium AZ31B-H24 Stiffness against density 1k 10k 10 100 1k Density (kg/m³) Yield strength (MPa) Plastic PLA Plastic PETG Plastic ABS Plastic TPU Plastic Nylon Rubber Aluminum Steel Iron Titanium Steel AISI 1018 Stainless Steel 304 Stainless Steel 316 Aluminum 6061-T6 Aluminum 7075-T6 Brass C360 Copper C110 Glass Steel AISI 1045 Steel AISI 4340 Steel A992 Stainless Steel 303 Stainless Steel 17-4PH Aluminum 5052-H32 Aluminum 7050-T7451 Titanium Ti-6Al-4V Brass C260 Nickel Inconel 718 Zinc Zamak 3 Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic POM/Acetal Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic PTFE Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA FDM ASA FDM Polycarbonate FDM PAHT-CF FDM HIPS SLA Resin Tough 2000 SLA Resin Elastic 50A SLS PA12 Nylon DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel Brick PCB Laminate FR-4 Silicon Ceramic Alumina 96% Aluminum A380 Aluminum 6063-T6 Aluminum 1100-O Aluminum ADC12 Magnesium AZ91D Solder SAC305 Plastic PBT GF30 Plastic PPS GF40 Plastic LCP GF30 Aluminum 2024-T351 Magnesium AZ31B-H24 Strength against density