Mechanical
Yield strength150MPasourcetypical, 0.2% tensile yield, ambient temperature
Ultimate tensile strength230MPasourcetypical, ambient temperature
Elongation at break3%sourcetypical, ambient temperature
Young's modulus (stiffness)45GPasourcetypical
Density1,810kg/m³sourcetypical
Strength to weight82.9kN·m/kg
Stiffness to weight24.9MN·m/kg
Poisson's ratio0.35sourcebase material: AZ91C casting (MIL-HDBK-5J handbook physical constant)
Shear modulus16.7GPa
Bulk modulus50GPa
Speed of sound4,986m/s
Thermal
Thermal conductivity72W/m·Ksourcetypical
Thermal expansion25µm/m·Ksourcetypical, temperature range not stated
100 mm part over a 50 °C swing125µm growth
Specific heat1,050J/kg·Ksourcetypical
Heats up and cools (diffusivity)37.9mm²/s
Thermal shock resistance6,240W/m
Melting point470–595°Csourcemelting range
Values forELEKTRON AZ91D magnesium die-casting alloy, as cast; Magnesium Elektron datasheet 475 (7/01), typical properties; Poisson from MIL-HDBK-5J for AZ91C castings.

Among 72 materials

1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum ADC12Solder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Magnesium AZ91D
Stiffness against density
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum ADC12Solder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Magnesium AZ91D
Strength against density

Compare Magnesium AZ91D with