Materials / Compare

Magnesium AZ31B-H24 vs. Stainless Steel 303

Compare Magnesium AZ31B-H24 vs. Stainless Steel 303 strength, stiffness, weight and thermal properties.

Magnesium AZ31B-H24Wrought
Stainless Steel 303Wrought
MechanicalMagnesium AZ31B-H24Stainless Steel 303
Yield strength220MPa1Outokumpu typical275MPa225% stronger
Ultimate tensile strength290MPa1Outokumpu typical585MPa22.02x stronger
Elongation at break13%1Outokumpu typical35%22.69x more ductile
Young's modulus (stiffness)44.8GPa3at RT200GPa24.46x stiffer
Density1,769kg/m³34.47x lighterat RT7,900kg/m³2
Strength to weight124kN·m/kg3.57x higher34.8kN·m/kg
Stiffness to weight25.3MN·m/kg25.3MN·m/kg
Poisson's ratio0.353design value0.34
Shear modulus16.6GPa76.9GPa4.64x stiffer in shear
Bulk modulus49.8GPa167GPa3.35x higher
Speed of sound5,032m/s5,032m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Magnesium AZ31B-H24Stainless Steel 303
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Magnesium AZ31B-H24Stainless Steel 303
Strength against densityHigher and further left: stronger for its weight
ThermalMagnesium AZ31B-H24Stainless Steel 303
Thermal conductivity76.9W/m·K15.13x more heat through a finat RT15W/m·K2
Thermal expansion26.8µm/m·K1mean16µm/m·K21.68x less
100 mm part over a 50 °C swing134µm growth80µm growth1.68x less
Specific heat1,040J/kg·K12.08x higherat RT500J/kg·K2
Heats up and cools (diffusivity)41.8mm²/s11x faster3.8mm²/s
Thermal shock resistance9,159W/m10.2x more resistant902W/m
Max service temperature149°C3continuous871°C5722 °C hotter
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Magnesium AZ31B-H24Stainless Steel 303
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Magnesium AZ31B-H24Stainless Steel 303
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources5 documents: Magnesium Elektron, Outokumpu, U.S. Department of Defense, Steel Construction Institute, Carpenter Technology
Magnesium AZ31B-H24
AZ31B-H24 sheet 0.016-0.062 in., MIL-HDBK-5J Table 4.2.1.0(b) (AMS 4377); strengths are S-basis MINIMUMS
Stainless Steel 303
1.4305 / UNS S30300, Outokumpu typical values (hot rolled, solution annealed) from 'Steel Grades, Properties and Global Standards'; max service from Carpenter CarTech 303 datasheet
  1. 1
    Elektron AZ31B Sheet, Plate & Coil (Datasheet 482)Magnesium Elektronarchived copyMagnesium AZ31B-H24 · Yield strength: typical, H24, 0.5-6 mm, 0.2 % proof stressMagnesium AZ31B-H24 · Ultimate tensile strength: typical, H24, 0.5-6 mmMagnesium AZ31B-H24 · Elongation at break: typical, H24, 0.5-6 mm, gauge 5.65√AMagnesium AZ31B-H24 · Thermal conductivity: typical (temper/temperature not stated)Magnesium AZ31B-H24 · Thermal expansion: typical (temperature range not stated)Magnesium AZ31B-H24 · Specific heat: typical
  2. 2
    Steel Grades, Properties and Global StandardsOutokumpuarchived copyStainless Steel 303 · Yield strength: Outokumpu typical (product P = hot rolled plate, transverse)Stainless Steel 303 · Ultimate tensile strength: Outokumpu typicalStainless Steel 303 · Elongation at break: Outokumpu typical, A5Stainless Steel 303 · Young's modulus (stiffness): at RT (Table 12)Stainless Steel 303 · Density: at RTStainless Steel 303 · Thermal conductivity: at RTStainless Steel 303 · Thermal expansion: mean, 20–100 °CStainless Steel 303 · Specific heat: at RT
  3. 3
    MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseMagnesium AZ31B-H24 · Young's modulus (stiffness): typical (handbook physical constant)Magnesium AZ31B-H24 · Density: nominalMagnesium AZ31B-H24 · Poisson's ratio: typical (handbook physical constant)Magnesium AZ31B-H24 · Max service temperature: stated application limit
  4. 4
    Design Manual for Structural Stainless Steel, 4th Edition (P413)Steel Construction Institutearchived copyStainless Steel 303 · Poisson's ratio: design value (structural stainless steels)
  5. 5
    Carpenter Stainless Type 303 Data SheetCarpenter Technologyarchived copyStainless Steel 303 · Max service temperature: continuous, scaling limit

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Questions

Mechanical

Is Magnesium AZ31B-H24 stronger than Stainless Steel 303?

Stainless Steel 303 is stronger: its yield strength is 275 MPa against 220 MPa for Magnesium AZ31B-H24 (25%).

Which is lighter, Magnesium AZ31B-H24 or Stainless Steel 303?

Magnesium AZ31B-H24 is lighter: 1,769 kg/m³ against 7,900 kg/m³ for Stainless Steel 303.

Which is stiffer, Magnesium AZ31B-H24 or Stainless Steel 303?

Stainless Steel 303 is stiffer: Young's modulus 200 GPa against 44.8 GPa for Magnesium AZ31B-H24, so the same part in Stainless Steel 303 deflects less under the same load.

Which is lighter for the same job, Magnesium AZ31B-H24 or Stainless Steel 303?

For the same stiffness or strength: Magnesium AZ31B-H24 is lighter for a stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.

Part that must beMagnesium AZ31B-H24Stainless Steel 303
Stiff rod or tie (tension)about equalabout equal
Stiff beam (bending)lighter2.11x heavier
Stiff panel or platelighter2.71x heavier
Strong rod or tielighter3.57x heavier
Strong beamlighter3.85x heavier
Strong panel or platelighter3.99x heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Magnesium AZ31B-H24 or Stainless Steel 303?

Stainless Steel 303 stretches further before it breaks: 35% elongation at break against 13% for Magnesium AZ31B-H24.

Thermal

Which handles higher temperatures, Magnesium AZ31B-H24 or Stainless Steel 303?

Stainless Steel 303 does: 871 °C against 149 °C for Magnesium AZ31B-H24.

Which conducts heat better, Magnesium AZ31B-H24 or Stainless Steel 303?

Magnesium AZ31B-H24 conducts heat better: 76.9 W/m·K against 15 W/m·K for Stainless Steel 303.

Which expands less with temperature?

Stainless Steel 303 expands less: 16 µm/m·K against 26.8 µm/m·K for Magnesium AZ31B-H24.

Related comparisons