Materials / Compare

Plastic ABS (bulk/injection) vs. Plastic PTFE

Compare Plastic ABS (bulk/injection) vs. Plastic PTFE strength, stiffness, weight and thermal properties.

Change either side
Plastic ABS (bulk/injection)Bulk polymer (molded or machined)
Plastic PTFEBulk polymer (molded or machined)
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Mechanical
Yield strength45MPasourcetypical, tensile stress at yield 23 °C9MPasourcetypical yield strength at 23 °C (Teflon PTFE, Table 8)
Ultimate tensile strengthnot sourced39.3MPasourcetypical, skived tape 0.13 mm
Flexural strength65MPasourcetypical, 23 °Cnot sourced
Elongation at break10%sourcenominal strain at break, 23 °C350%sourcetypical, skived tape 0.13 mm
Young's modulus (stiffness)2.3GPasourcetypicalnot sourced
Density1,040kg/m³sourcetypical2,160kg/m³sourcetypical (standard specific gravity, ASTM D4894)
Strength to weight43.3kN·m/kg10.4x higher4.17kN·m/kg
Stiffness to weight2.21MN·m/kgnot sourced
Poisson's ratio0.39sourcetypical, ABS family (Covestro Part and Mold Design guide, Table 3-1)0.46sourcetypical, 23 °C (Teflon PTFE resins, Chemours handbook)
Shear modulus0.827GPanot sourced
Bulk modulus3.48GPanot sourced
Speed of sound1,487m/snot sourced
Thermal
Thermal conductivity0.17W/m·Ksourcetypical0.25W/m·Ksourcetypical, granular resin, 4.6 mm specimen
Thermal expansion80–110µm/m·Ksourcerange100µm/m·Ksourcetypical, granular resin, 23-60 °C (ASTM E228)
100 mm part over a 50 °C swing475µm growth5% less500µm growth
Specific heatnot sourced1,400J/kg·Ksourcetypical, granular resin, 20 °C (ASTM D4591)
Heats up and cools (diffusivity)not sourced0.0827mm²/s
Thermal shock resistance21.4W/mnot sourced
Melting pointnot sourced327°Csourcesecond melting peak (sintered polymer), +/-10
Max service temperature94°CsourceHDT 1.8 MPa (annealed 4 h/80 °C)260°Csourceservice temperature (Chemours general Teflon PTFE statement)
Values forINEOS Styrolution Terluran GP-22 general-purpose injection-molding ABS, ISO typical values (TDS revision 08/01/2022)Chemours Teflon PTFE 7C X granular molding resin, typical values (tensile/elongation measured on 0.13 mm skived tape)

Every value links to the document that states it. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Questions

Is Plastic ABS (bulk/injection) stronger than Plastic PTFE?

Plastic ABS (bulk/injection) is stronger: its yield strength is 45 MPa against 9 MPa for Plastic PTFE (5x).

Which is lighter, Plastic ABS (bulk/injection) or Plastic PTFE?

Plastic ABS (bulk/injection) is lighter: 1,040 kg/m³ against 2,160 kg/m³ for Plastic PTFE.

Which is lighter for the same job, Plastic ABS (bulk/injection) or Plastic PTFE?

For the same stiffness or strength: Plastic ABS (bulk/injection) is lighter for a strong rod or tie, strong beam, strong panel or plate.

Part that must bePlastic ABS (bulk/injection)Plastic PTFE
Strong rod or tielighter10.4x heavier
Strong beamlighter6.07x heavier
Strong panel or platelighter4.64x heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which conducts heat better, Plastic ABS (bulk/injection) or Plastic PTFE?

Plastic PTFE conducts heat better: 0.25 W/m·K against 0.17 W/m·K for Plastic ABS (bulk/injection).

Which expands less with temperature?

Plastic ABS (bulk/injection) expands less: 95 µm/m·K against 100 µm/m·K for Plastic PTFE.

Among 59 materials

1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelPlastic ABS (bulk/injection)
Stiffness against density
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPlastic ABS (bulk/injection)Plastic PTFE
Strength against density