Materials / Plastic

Plastic ABS (bulk/injection)

Plastic ABS (bulk/injection) (bulk/injection) strength, stiffness, density and thermal properties, with their source.

A bracket in Plastic ABS (bulk/injection), smooth finish.

ProcessBulk polymer (molded or machined)
Mechanical
Yield strength45MPasourcetypical, tensile stress at yield 23 °C
Ultimate tensile strengthnot sourced
Flexural strength65MPasourcetypical, 23 °C
Elongation at break10%sourcenominal strain at break, 23 °C
Young's modulus (stiffness)2.3GPasourcetypical
Density1,040kg/m³sourcetypical
Strength to weight43.3kN·m/kg
Stiffness to weight2.21MN·m/kg
Poisson's ratio0.39sourcetypical, ABS family (Covestro Part and Mold Design guide, Table 3-1)
Shear modulus0.827GPa
Bulk modulus3.48GPa
Speed of sound1,487m/s
Thermal
Thermal conductivity0.17W/m·Ksourcetypical
Thermal expansion80–110µm/m·Ksourcerange
100 mm part over a 50 °C swing475µm growth
Specific heatnot sourced
Heats up and cools (diffusivity)not sourced
Thermal shock resistance21.4W/m
Max service temperature94°CsourceHDT 1.8 MPa (annealed 4 h/80 °C)
Values forINEOS Styrolution Terluran GP-22 general-purpose injection-molding ABS, ISO typical values (TDS revision 08/01/2022)

Among 59 materials

1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelPlastic ABS (bulk/injection)
Stiffness against density
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPlastic ABS (bulk/injection)
Strength against density

Compare Plastic ABS (bulk/injection) with