Materials / Compare

Plastic ABS vs. Wood

Compare Plastic ABS vs. Wood strength, stiffness, weight and thermal properties.

Plastic ABS3D printed (FDM)
WoodNatural
MechanicalPlastic ABSWood
Yield strength38.1MPa1not given (tensile used)
Ultimate tensile strength38.1MPa1modulus of rupture99MPa2
Compressive strengthnot sourced46.6MPa2
Flexural strength61.1MPa1modulus of rupture99MPa2
Elongation at break4.6%1not sourced
Young's modulus (stiffness)1.96GPa1bending MOE12.5GPa26.37x stiffer
Density1,100kg/m³1681–702kg/m³3
Strength to weight34.6kN·m/kg143kN·m/kg4.13x higher
Stiffness to weight1.78MN·m/kg18.1MN·m/kg10.1x higher
Poisson's ratiobase material0.394mu_LR0.352
Shear modulus0.706GPa4.63GPa6.56x stiffer in shear
Bulk modulus2.97GPa13.9GPa4.67x higher
Speed of sound1,336m/s4,252m/s3.18x faster
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic TPUPlastic NylonAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic ABSWood
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic TPUPlastic NylonRubberAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic ABSWood
Strength against densityHigher and further left: stronger for its weight
ThermalPlastic ABSWood
Thermal conductivitybase material0.17W/m·K5across grain0.18W/m·K6
Thermal expansionbase material80–110µm/m·K5parallel to grain3.1–4.5µm/m·K6
100 mm part over a 50 °C swing475µm growth19µm growth25x less
Specific heatnot sourcedsolid wood1,700J/kg·K6
Heats up and cools (diffusivity)not sourced0.153mm²/s
Thermal shock resistance21.2W/m244W/m11.5x more resistant
Glass transition101°C1not sourced
Max service temperatureHDT 0.455 MPa86.6°C1not sourced
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic NylonRubberAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic ABSWood
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic NylonAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic ABSWood
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources6 documents: UltiMaker, USDA Forest Products Laboratory, Covestro, INEOS Styrolution
Plastic ABS
Ultimaker ABS, 3D-printed specimens, XY (flat); Ultimaker S5 Pro, engineering intent profile, 0.15 mm layer height, AA 0.4 print core, 100% infill, Cura 4.9, printed one-at-a-time, conditioned >=24 h at room temperature. TDS v5.00, April 20, 2022.
Wood
Northern red oak (Quercus rubra), clear straight-grained specimens at 12% MC, parallel to grain unless stated; USDA FPL Wood Handbook FPL-GTR-282 (2021) Ch. 4 and Ch. 5
  1. 1
    Ultimaker ABS Technical Data Sheet, v5.00UltiMakerarchived copyPlastic ABS · Yield strength: typicalPlastic ABS · Ultimate tensile strength: typical, peak stress (= stress at yield)Plastic ABS · Flexural strength: typicalPlastic ABS · Elongation at break: typicalPlastic ABS · Young's modulus (stiffness): typicalPlastic ABS · Density: typicalPlastic ABS · Glass transition: typicalPlastic ABS · Max service temperature: HDT 0.455 MPa (printed specimens)
  2. 2
    Wood Handbook (FPL-GTR-282), Chapter 5: Mechanical Properties of WoodUSDA Forest Products LaboratoryWood · Ultimate tensile strength: modulus of rupture (no direct tensile value)Wood · Compressive strength: compression parallel to grain (maximum crushing strength), 12% MCWood · Flexural strength: modulus of rupture (static bending), 12% MCWood · Young's modulus (stiffness): bending MOE, parallel to grainWood · Poisson's ratio: mu_LR (red oak group, ~12% MC)
  3. 3
    Technical Note 218: Weights of Various Woods Grown in the United States (1953)USDA Forest Products LaboratoryWood · Density: average weight of clear wood at 8% and 15% moisture content
  4. 4
    Engineering Polymers Part and Mold Design: Thermoplastics, A Design GuideCovestroarchived copyPlastic ABS · Poisson's ratio: base material: ABS family typical (Covestro Part and Mold Design guide, Table 3-1)
  5. 5
    Terluran GP-22 (ABS) Product Data SheetINEOS StyrolutionPlastic ABS · Thermal conductivity: base material: INEOS Styrolution Terluran GP-22 injection-molding ABS, typicalPlastic ABS · Thermal expansion: base material: INEOS Styrolution Terluran GP-22 injection-molding ABS, range
  6. 6
    Wood Handbook (FPL-GTR-282), Chapter 4: Moisture Relations and Physical Properties of WoodUSDA Forest Products LaboratoryWood · Thermal conductivity: across grain, 12% MC (Table 4-7, approximate)Wood · Thermal expansion: parallel to grain, ovendry wood, range across speciesWood · Specific heat: solid wood (all species), 12% MC, 27 C

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Plastic ABS is 3D printed: its properties depend on build direction and print settings; these are typical values.

Questions

Mechanical

Is Plastic ABS stronger than Wood?

Wood is stronger: its tensile strength is 99 MPa against yield strength 38.1 MPa for Plastic ABS (2.6x).

Which is lighter, Plastic ABS or Wood?

Wood is lighter: 692 kg/m³ against 1,100 kg/m³ for Plastic ABS.

Which is stiffer, Plastic ABS or Wood?

Wood is stiffer: Young's modulus 12.5 GPa against 1.96 GPa for Plastic ABS, so the same part in Wood deflects less under the same load.

Which is lighter for the same job, Plastic ABS or Wood?

For the same stiffness or strength: Wood is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.

Part that must bePlastic ABSWood
Stiff rod or tie (tension)10.1x heavierlighter
Stiff beam (bending)4.02x heavierlighter
Stiff panel or plate2.95x heavierlighter
Strong rod or tie4.13x heavierlighter
Strong beam3.01x heavierlighter
Strong panel or plate2.56x heavierlighter

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Thermal

Which conducts heat better, Plastic ABS or Wood?

Wood conducts heat better: 0.18 W/m·K against 0.17 W/m·K for Plastic ABS.

Which expands less with temperature?

Wood expands less: 3.8 µm/m·K against 95 µm/m·K for Plastic ABS.