Materials / Plastic

Plastic ABS

Plastic ABS strength, stiffness, density and thermal properties, with their source.

A bracket in Plastic ABS, 3D-printed (layer lines) finish.

Process3D printed (FDM)
Mechanical
Yield strength38.1MPasourcetypical
Ultimate tensile strength38.1MPasourcetypical, peak stress (= stress at yield)
Flexural strength61.1MPasourcetypical
Elongation at break4.6%sourcetypical
Young's modulus (stiffness)1.96GPasourcetypical
Density1,100kg/m³sourcetypical
Strength to weight34.6kN·m/kg
Stiffness to weight1.78MN·m/kg
Poisson's ratio0.39sourcebase material: ABS family typical (Covestro Part and Mold Design guide, Table 3-1)
Shear modulus0.706GPa
Bulk modulus2.97GPa
Speed of sound1,336m/s
Thermal
Thermal conductivity0.17W/m·Ksourcebase material: INEOS Styrolution Terluran GP-22 injection-molding ABS, typical
Thermal expansion80–110µm/m·Ksourcebase material: INEOS Styrolution Terluran GP-22 injection-molding ABS, range
100 mm part over a 50 °C swing475µm growth
Specific heatnot sourced
Heats up and cools (diffusivity)not sourced
Thermal shock resistance21.2W/m
Glass transition101°Csourcetypical
Max service temperature86.6°CsourceHDT 0.455 MPa (printed specimens)
Values forUltimaker ABS, 3D-printed specimens, XY (flat); Ultimaker S5 Pro, engineering intent profile, 0.15 mm layer height, AA 0.4 print core, 100% infill, Cura 4.9, printed one-at-a-time, conditioned >=24 h at room temperature. TDS v5.00, April 20, 2022.

Plastic ABS is 3D printed: its properties depend on build direction and print settings; these are typical values.

Among 59 materials

1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic TPUPlastic NylonAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelPlastic ABS
Stiffness against density
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic TPUPlastic NylonRubberAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPlastic ABS
Strength against density

Compare Plastic ABS with