Mechanical
Yield strength38.1MPasourcetypical9MPasourcetypical yield strength at 23 °C (Teflon PTFE, Table 8)
Ultimate tensile strength38.1MPasourcetypical, peak stress (= stress at yield)39.3MPasourcetypical, skived tape 0.13 mm
Flexural strength61.1MPasourcetypicalnot sourced
Elongation at break4.6%sourcetypical350%sourcetypical, skived tape 0.13 mm
Young's modulus (stiffness)1.96GPasourcetypicalnot sourced
Density1,100kg/m³sourcetypical2,160kg/m³sourcetypical (standard specific gravity, ASTM D4894)
Strength to weight34.6kN·m/kg8.31x higher4.17kN·m/kg
Stiffness to weight1.78MN·m/kgnot sourced
Poisson's ratio0.39sourcebase material: ABS family typical (Covestro Part and Mold Design guide, Table 3-1)0.46sourcetypical, 23 °C (Teflon PTFE resins, Chemours handbook)
Shear modulus0.706GPanot sourced
Bulk modulus2.97GPanot sourced
Speed of sound1,336m/snot sourced
Thermal
Thermal conductivity0.17W/m·Ksourcebase material: INEOS Styrolution Terluran GP-22 injection-molding ABS, typical0.25W/m·Ksourcetypical, granular resin, 4.6 mm specimen
Thermal expansion80–110µm/m·Ksourcebase material: INEOS Styrolution Terluran GP-22 injection-molding ABS, range100µm/m·Ksourcetypical, granular resin, 23-60 °C (ASTM E228)
100 mm part over a 50 °C swing475µm growth5% less500µm growth
Specific heatnot sourced1,400J/kg·Ksourcetypical, granular resin, 20 °C (ASTM D4591)
Heats up and cools (diffusivity)not sourced0.0827mm²/s
Thermal shock resistance21.2W/mnot sourced
Melting pointnot sourced327°Csourcesecond melting peak (sintered polymer), +/-10
Glass transition101°Csourcetypicalnot sourced
Max service temperature86.6°CsourceHDT 0.455 MPa (printed specimens)260°Csourceservice temperature (Chemours general Teflon PTFE statement)
Values forUltimaker ABS, 3D-printed specimens, XY (flat); Ultimaker S5 Pro, engineering intent profile, 0.15 mm layer height, AA 0.4 print core, 100% infill, Cura 4.9, printed one-at-a-time, conditioned >=24 h at room temperature. TDS v5.00, April 20, 2022.Chemours Teflon PTFE 7C X granular molding resin, typical values (tensile/elongation measured on 0.13 mm skived tape)

Every value links to the document that states it. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Plastic ABS is 3D printed: its properties depend on build direction and print settings; these are typical values.

Questions

Is Plastic ABS stronger than Plastic PTFE?

Plastic ABS is stronger: its yield strength is 38.1 MPa against 9 MPa for Plastic PTFE (4.23x).

Which is lighter, Plastic ABS or Plastic PTFE?

Plastic ABS is lighter: 1,100 kg/m³ against 2,160 kg/m³ for Plastic PTFE.

Which is lighter for the same job, Plastic ABS or Plastic PTFE?

For the same stiffness or strength: Plastic ABS is lighter for a strong rod or tie, strong beam, strong panel or plate.

Part that must bePlastic ABSPlastic PTFE
Strong rod or tielighter8.31x heavier
Strong beamlighter5.14x heavier
Strong panel or platelighter4.04x heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which conducts heat better, Plastic ABS or Plastic PTFE?

Plastic PTFE conducts heat better: 0.25 W/m·K against 0.17 W/m·K for Plastic ABS.

Which expands less with temperature?

Plastic ABS expands less: 95 µm/m·K against 100 µm/m·K for Plastic PTFE.

Among 59 materials

1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic TPUPlastic NylonAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelPlastic ABS
Stiffness against density
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic TPUPlastic NylonRubberAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPlastic ABSPlastic PTFE
Strength against density

Related comparisons