Materials / Compare

Plastic Nylon PA6 vs. Stainless Steel 303

Compare Plastic Nylon PA6 vs. Stainless Steel 303 strength, stiffness, weight and thermal properties.

Plastic Nylon PA6Bulk polymer (molded or machined)
Stainless Steel 303Wrought
MechanicalPlastic Nylon PA6Stainless Steel 303
Yield strength90MPa1Outokumpu typical275MPa23.06x stronger
Ultimate tensile strengthnot stated (yield given)Outokumpu typical585MPa2
Elongation at break10%1Outokumpu typical35%23.5x more ductile
Young's modulus (stiffness)3.5GPa1at RT200GPa257.1x stiffer
Density1,130kg/m³16.99x lighterat RT7,900kg/m³2
Strength to weight79.6kN·m/kg2.29x higher34.8kN·m/kg
Stiffness to weight3.1MN·m/kg25.3MN·m/kg8.17x higher
Poisson's ratiobase material0.43design value0.34
Shear modulus1.25GPa76.9GPa61.5x stiffer in shear
Bulk modulus5.83GPa167GPa28.6x higher
Speed of sound1,760m/s5,032m/s2.86x faster
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic Nylon PA6Stainless Steel 303
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic Nylon PA6Stainless Steel 303
Strength against densityHigher and further left: stronger for its weight
ThermalPlastic Nylon PA6Stainless Steel 303
Thermal conductivity0.33W/m·K1at RT15W/m·K245.5x more heat through a fin
Thermal expansionlongitudinal102µm/m·K1mean16µm/m·K26.38x less
100 mm part over a 50 °C swing510µm growth80µm growth6.38x less
Specific heat1,700J/kg·K13.4x higherat RT500J/kg·K2
Heats up and cools (diffusivity)0.172mm²/s3.8mm²/s22.1x faster
Thermal shock resistance49.9W/m902W/m18.1x more resistant
Melting pointDSC220°C1not sourced
Max service temperature87°C1continuous871°C5784 °C hotter
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic Nylon PA6Stainless Steel 303
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic Nylon PA6Stainless Steel 303
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources5 documents: BASF, Outokumpu, Covestro, Steel Construction Institute, Carpenter Technology
Plastic Nylon PA6
BASF Ultramid B3S (PA6, unreinforced injection-moulding grade), Product Information 02/2026, dry values (ISO methods)
Stainless Steel 303
1.4305 / UNS S30300, Outokumpu typical values (hot rolled, solution annealed) from 'Steel Grades, Properties and Global Standards'; max service from Carpenter CarTech 303 datasheet
  1. 1
    Ultramid B3S Product InformationBASFPlastic Nylon PA6 · Yield strength: typical, dryPlastic Nylon PA6 · Elongation at break: nominal strain at break, dryPlastic Nylon PA6 · Young's modulus (stiffness): typical, dryPlastic Nylon PA6 · Density: typicalPlastic Nylon PA6 · Thermal conductivity: typicalPlastic Nylon PA6 · Thermal expansion: longitudinal, 23-55 °CPlastic Nylon PA6 · Specific heat: typicalPlastic Nylon PA6 · Melting point: DSCPlastic Nylon PA6 · Max service temperature: IEC 60216 temperature index, 20000 h
  2. 2
    Steel Grades, Properties and Global StandardsOutokumpuarchived copyStainless Steel 303 · Yield strength: Outokumpu typical (product P = hot rolled plate, transverse)Stainless Steel 303 · Ultimate tensile strength: Outokumpu typicalStainless Steel 303 · Elongation at break: Outokumpu typical, A5Stainless Steel 303 · Young's modulus (stiffness): at RT (Table 12)Stainless Steel 303 · Density: at RTStainless Steel 303 · Thermal conductivity: at RTStainless Steel 303 · Thermal expansion: mean, 20–100 °CStainless Steel 303 · Specific heat: at RT
  3. 3
    Engineering Polymers Part and Mold Design: Thermoplastics, A Design GuideCovestroPlastic Nylon PA6 · Poisson's ratio: base material: unfilled polyamide (PA), conditioned, maker design-guide family value (Covestro Table 3-1)
  4. 4
    Design Manual for Structural Stainless Steel, 4th Edition (P413)Steel Construction Institutearchived copyStainless Steel 303 · Poisson's ratio: design value (structural stainless steels)
  5. 5
    Carpenter Stainless Type 303 Data SheetCarpenter Technologyarchived copyStainless Steel 303 · Max service temperature: continuous, scaling limit

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Questions

Mechanical

Is Plastic Nylon PA6 stronger than Stainless Steel 303?

Stainless Steel 303 is stronger: its yield strength is 275 MPa against 90 MPa for Plastic Nylon PA6 (3.06x).

Which is lighter, Plastic Nylon PA6 or Stainless Steel 303?

Plastic Nylon PA6 is lighter: 1,130 kg/m³ against 7,900 kg/m³ for Stainless Steel 303.

Which is stiffer, Plastic Nylon PA6 or Stainless Steel 303?

Stainless Steel 303 is stiffer: Young's modulus 200 GPa against 3.5 GPa for Plastic Nylon PA6, so the same part in Stainless Steel 303 deflects less under the same load.

Which is lighter for the same job, Plastic Nylon PA6 or Stainless Steel 303?

For the same stiffness or strength: Plastic Nylon PA6 is lighter for a stiff panel or plate, strong rod or tie, strong beam, strong panel or plate; Stainless Steel 303 is lighter for a stiff rod or tie (tension), stiff beam (bending).

Part that must bePlastic Nylon PA6Stainless Steel 303
Stiff rod or tie (tension)8.17x heavierlighter
Stiff beam (bending)8% heavierlighter
Stiff panel or platelighter1.82x heavier
Strong rod or tielighter2.29x heavier
Strong beamlighter3.32x heavier
Strong panel or platelighter4x heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Plastic Nylon PA6 or Stainless Steel 303?

Stainless Steel 303 stretches further before it breaks: 35% elongation at break against 10% for Plastic Nylon PA6.

Thermal

Which handles higher temperatures, Plastic Nylon PA6 or Stainless Steel 303?

Stainless Steel 303 does: 871 °C against 87 °C for Plastic Nylon PA6.

Which conducts heat better, Plastic Nylon PA6 or Stainless Steel 303?

Stainless Steel 303 conducts heat better: 15 W/m·K against 0.33 W/m·K for Plastic Nylon PA6.

Which expands less with temperature?

Stainless Steel 303 expands less: 16 µm/m·K against 102 µm/m·K for Plastic Nylon PA6.