Materials / Compare

Plastic PLA vs. Plastic PTFE

Compare Plastic PLA vs. Plastic PTFE strength, stiffness, weight and thermal properties.

Change either side
Plastic PLA3D printed (FDM)
Plastic PTFEBulk polymer (molded or machined)
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Mechanical
Yield strength52.5MPasourcetypical9MPasourcetypical yield strength at 23 °C (Teflon PTFE, Table 8)
Ultimate tensile strength52.5MPasourcetypical, peak stress (= stress at yield)39.3MPasourcetypical, skived tape 0.13 mm
Flexural strength96.8MPasourcetypicalnot sourced
Elongation at break7.8%sourcetypical350%sourcetypical, skived tape 0.13 mm
Young's modulus (stiffness)3.25GPasourcetypicalnot sourced
Density1,240kg/m³sourcetypical2,160kg/m³sourcetypical (standard specific gravity, ASTM D4894)
Strength to weight42.3kN·m/kg10.2x higher4.17kN·m/kg
Stiffness to weight2.62MN·m/kgnot sourced
Poisson's rationot sourced0.46sourcetypical, 23 °C (Teflon PTFE resins, Chemours handbook)
Shear modulusnot sourcednot sourced
Bulk modulusnot sourcednot sourced
Speed of sound1,619m/snot sourced
Thermal
Thermal conductivity0.13W/m·Ksourcebase material: NatureWorks Ingeo biopolymer, amorphous sheet, 25 °C0.25W/m·Ksourcetypical, granular resin, 4.6 mm specimen
Thermal expansionnot sourced100µm/m·Ksourcetypical, granular resin, 23-60 °C (ASTM E228)
100 mm part over a 50 °C swingnot sourced500µm growth
Specific heat1,200J/kg·Ksourcebase material: NatureWorks Ingeo biopolymer, amorphous sheet, 25 °C1,400J/kg·Ksourcetypical, granular resin, 20 °C (ASTM D4591)
Heats up and cools (diffusivity)0.0874mm²/s6% faster0.0827mm²/s
Thermal shock resistancenot sourcednot sourced
Melting point152°Csourcetypical327°Csourcesecond melting peak (sintered polymer), +/-10
Glass transition59.1°Csourcetypicalnot sourced
Max service temperature58.8°CsourceHDT 0.455 MPa (printed specimens)260°Csourceservice temperature (Chemours general Teflon PTFE statement)
Values forUltimaker PLA, 3D-printed specimens, XY (flat) orientation; Ultimaker S5 Pro, engineering intent profile, 0.15 mm layer height, AA 0.4 print core, 100% infill, Cura 4.9, printed one-at-a-time, conditioned >=24 h at room temperature. TDS dated April 20, 2022.Chemours Teflon PTFE 7C X granular molding resin, typical values (tensile/elongation measured on 0.13 mm skived tape)

Every value links to the document that states it. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Plastic PLA is 3D printed: its properties depend on build direction and print settings; these are typical values.

Questions

Is Plastic PLA stronger than Plastic PTFE?

Plastic PLA is stronger: its yield strength is 52.5 MPa against 9 MPa for Plastic PTFE (5.83x).

Which is lighter, Plastic PLA or Plastic PTFE?

Plastic PLA is lighter: 1,240 kg/m³ against 2,160 kg/m³ for Plastic PTFE.

Which is lighter for the same job, Plastic PLA or Plastic PTFE?

For the same stiffness or strength: Plastic PLA is lighter for a strong rod or tie, strong beam, strong panel or plate.

Part that must bePlastic PLAPlastic PTFE
Strong rod or tielighter10.2x heavier
Strong beamlighter5.64x heavier
Strong panel or platelighter4.21x heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which conducts heat better, Plastic PLA or Plastic PTFE?

Plastic PTFE conducts heat better: 0.25 W/m·K against 0.13 W/m·K for Plastic PLA.

Among 59 materials

1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PETGPlastic ABSPlastic TPUPlastic NylonAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelPlastic PLA
Stiffness against density
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PETGPlastic ABSPlastic TPUPlastic NylonRubberAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPlastic PLAPlastic PTFE
Strength against density

Related comparisons