Materials / Compare

Plastic POM/Acetal vs. Steel AISI 1018

Compare Plastic POM/Acetal vs. Steel AISI 1018 strength, stiffness, weight and thermal properties.

Plastic POM/AcetalBulk polymer (molded or machined)
Steel AISI 1018Wrought
MechanicalPlastic POM/AcetalSteel AISI 1018
Yield strength69MPa1producer-stated372MPa25.39x stronger
Ultimate tensile strength69MPa1producer-stated441MPa26.39x stronger
Compressive strength124MPa1not sourced
Flexural strength99MPa1not sourced
Elongation at break75%15x more ductilein 2 in15%2
Young's modulus (stiffness)2.8GPa1base material200GPa3
Density1,420kg/m³4base material7,861kg/m³3
Strength to weight48.6kN·m/kg3% higher47.3kN·m/kg
Stiffness to weight1.97MN·m/kg25.4MN·m/kg12.9x higher
Poisson's ratio0.351base material0.323
Shear modulus1.04GPa75.7GPa73x stiffer in shear
Bulk modulus3.11GPa185GPa59.5x higher
Speed of sound1,404m/s5,043m/s3.59x faster
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumStainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic POM/AcetalSteel AISI 1018
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumStainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic POM/AcetalSteel AISI 1018
Strength against densityHigher and further left: stronger for its weight
ThermalPlastic POM/AcetalSteel AISI 1018
Thermal conductivity0.4W/m·K1base material51.9W/m·K3
Thermal expansionmean122µm/m·K1base material12µm/m·K510.2x less
100 mm part over a 50 °C swing610µm growth60µm growth10.2x less
Specific heataverage -18 to 100 °C1,465J/kg·K1base material486J/kg·K3
Heats up and cools (diffusivity)0.192mm²/s13.6mm²/s70.7x faster
Thermal shock resistance52.5W/m5,473W/m104x more resistant
Melting point175°C1not sourced
Max service temperatureHDT 1.8 MPa125°C1not sourced
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumStainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic POM/AcetalSteel AISI 1018
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumStainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic POM/AcetalSteel AISI 1018
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources5 documents: DuPont, Niagara LaSalle, U.S. Department of Defense, Ovako
Plastic POM/Acetal
DuPont Delrin 100 acetal homopolymer, Table 2 'Typical Properties of Delrin Acetal Resins' (ASTM methods), Delrin Design Guide Module III hosted on delrin.com
Steel AISI 1018
AISI 1018 cold drawn bar (Niagara LaSalle, cold-finished bar producer)
  1. 1
    Delrin Acetal Resin Design Guide, Module IIIDuPontarchived copyPlastic POM/Acetal · Yield strength: typical (single ASTM D638 tensile strength)Plastic POM/Acetal · Ultimate tensile strength: typicalPlastic POM/Acetal · Compressive strength: compressive stress at 10% deformationPlastic POM/Acetal · Flexural strength: flexural yield strength, typicalPlastic POM/Acetal · Elongation at break: typicalPlastic POM/Acetal · Young's modulus (stiffness): typicalPlastic POM/Acetal · Poisson's ratio: typicalPlastic POM/Acetal · Thermal conductivity: typicalPlastic POM/Acetal · Thermal expansion: mean, 29 to 60 °CPlastic POM/Acetal · Specific heat: average -18 to 100 °C, Delrin acetal resins (not grade-specific)Plastic POM/Acetal · Melting point: crystalline melting pointPlastic POM/Acetal · Max service temperature: HDT 1.8 MPa (annealed)
  2. 2
    1018 PropertiesNiagara LaSallearchived copySteel AISI 1018 · Yield strength: producer-stated, cold drawnSteel AISI 1018 · Ultimate tensile strength: producer-stated, cold drawnSteel AISI 1018 · Elongation at break: in 2 in (50.8 mm)
  3. 3
    MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseSteel AISI 1018 · Young's modulus (stiffness): base material: AISI 1025 plain carbon steel (MIL-HDBK-5J design value; ASTM A108 bar is the cold-finished carbon-steel bar spec that also covers 1018)Steel AISI 1018 · Density: base material: AISI 1025 plain carbon steel (MIL-HDBK-5J design value; ASTM A108 bar is the cold-finished carbon-steel bar spec that also covers 1018)Steel AISI 1018 · Poisson's ratio: base material: AISI 1025 plain carbon steel (MIL-HDBK-5J design value; ASTM A108 bar is the cold-finished carbon-steel bar spec that also covers 1018)Steel AISI 1018 · Thermal conductivity: base material: AISI 1025 plain carbon steel (MIL-HDBK-5J design value; ASTM A108 bar is the cold-finished carbon-steel bar spec that also covers 1018)Steel AISI 1018 · Specific heat: base material: AISI 1025 plain carbon steel (MIL-HDBK-5J design value; ASTM A108 bar is the cold-finished carbon-steel bar spec that also covers 1018)
  4. 4
    Delrin 100 Product Data SheetDuPontPlastic POM/Acetal · Density: typical (DuPont product information for Delrin 100 NC010; 'The data listed here fall within the normal range of product properties')
  5. 5
    S275JR Steel GradeOvakoSteel AISI 1018 · Thermal expansion: base material: unalloyed carbon steel, Ovako family table (S275JR, 'none alloyed structural steels', C <= 0.21%); mean 20-300 °C

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Questions

Mechanical

Is Plastic POM/Acetal stronger than Steel AISI 1018?

Steel AISI 1018 is stronger: its yield strength is 372 MPa against 69 MPa for Plastic POM/Acetal (5.39x).

Which is lighter, Plastic POM/Acetal or Steel AISI 1018?

Plastic POM/Acetal is lighter: 1,420 kg/m³ against 7,861 kg/m³ for Steel AISI 1018.

Which is stiffer, Plastic POM/Acetal or Steel AISI 1018?

Steel AISI 1018 is stiffer: Young's modulus 200 GPa against 2.8 GPa for Plastic POM/Acetal, so the same part in Steel AISI 1018 deflects less under the same load.

Which is lighter for the same job, Plastic POM/Acetal or Steel AISI 1018?

For the same stiffness or strength: Plastic POM/Acetal is lighter for a stiff panel or plate, strong rod or tie, strong beam, strong panel or plate; Steel AISI 1018 is lighter for a stiff rod or tie (tension), stiff beam (bending).

Part that must bePlastic POM/AcetalSteel AISI 1018
Stiff rod or tie (tension)12.9x heavierlighter
Stiff beam (bending)1.53x heavierlighter
Stiff panel or platelighter33% heavier
Strong rod or tielighter3% heavier
Strong beamlighter1.8x heavier
Strong panel or platelighter2.38x heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Plastic POM/Acetal or Steel AISI 1018?

Plastic POM/Acetal stretches further before it breaks: 75% elongation at break against 15% for Steel AISI 1018.

Thermal

Which conducts heat better, Plastic POM/Acetal or Steel AISI 1018?

Steel AISI 1018 conducts heat better: 51.9 W/m·K against 0.4 W/m·K for Plastic POM/Acetal.

Which expands less with temperature?

Steel AISI 1018 expands less: 12 µm/m·K against 122 µm/m·K for Plastic POM/Acetal.