Materials / Compare

SLA Resin Standard vs. Steel AISI 1045

Compare SLA Resin Standard vs. Steel AISI 1045 strength, stiffness, weight and thermal properties.

Change either side
SLA Resin Standard3D printed (SLA resin)
Steel AISI 1045Wrought
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Mechanical
Yield strengthnot given (tensile used)531MPasourceproducer-stated, cold drawn
Ultimate tensile strength60MPasourcetypical627MPasourceproducer-stated, cold drawn
Flexural strength105MPasourcetypicalnot sourced
Elongation at break8%sourcetypical12%sourcein 2 in (50.8 mm)
Young's modulus (stiffness)2.75GPasourcetypical210GPasourcetypical76.4x stiffer
Densitynot sourced7,800kg/m³sourcetypical
Strength to weightnot sourced68.1kN·m/kg
Stiffness to weightnot sourced26.9MN·m/kg
Poisson's rationot sourced0.3sourcetypical
Shear modulusnot sourced80.8GPa
Bulk modulusnot sourced175GPa
Speed of soundnot sourced5,189m/s
Thermal
Thermal conductivitynot sourced40–45W/m·Ksourcetypical range, ambient
Thermal expansionnot sourced12µm/m·Ksourcetypical, mean 20-300 °C
100 mm part over a 50 °C swingnot sourced60µm growth
Specific heatnot sourced460–480J/kg·Ksourcetypical range, 50/100 °C
Heats up and cools (diffusivity)not sourced11.6mm²/s
Thermal shock resistancenot sourced6,269W/m
Max service temperature59°CsourceHDT 1.8 MPanot sourced
Values forFormlabs Clear Resin V5 (FLGPCL05), TDS Rev. 01 March 20, 2024; printed on Form 4 at 100 µm, washed 5 min in >=99% IPA, post-cured 15 min at 60 °C in Form Cure. Orientation not stated.AISI 1045 cold drawn bar (Niagara LaSalle) for mechanical; Ovako C45 (lists 'SAE 1045' as a similar designation) for physical constants

Every value links to the document that states it. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

SLA Resin Standard is 3D printed: its properties depend on build direction and print settings; these are typical values.

Questions

Is SLA Resin Standard stronger than Steel AISI 1045?

Steel AISI 1045 is stronger: its yield strength is 531 MPa against tensile strength 60 MPa for SLA Resin Standard (8.85x).

Which is stiffer, SLA Resin Standard or Steel AISI 1045?

Steel AISI 1045 is stiffer: Young's modulus 210 GPa against 2.75 GPa for SLA Resin Standard, so the same part in Steel AISI 1045 deflects less under the same load.

Among 59 materials

1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonAluminumSteelIronTitaniumSteel AISI 1018Stainless 304Stainless 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 4340Steel A992Stainless 303Stainless 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelSteel AISI 1045
Stiffness against density
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberAluminumSteelIronTitaniumSteel AISI 1018Stainless 304Stainless 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 4340Steel A992Stainless 303Stainless 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickSteel AISI 1045
Strength against density