Materials / Compare

SLA Resin Standard vs. Steel AISI 1018

Compare SLA Resin Standard vs. Steel AISI 1018 strength, stiffness, weight and thermal properties.

SLA Resin Standard3D printed (SLA resin)
Steel AISI 1018Wrought
MechanicalSLA Resin StandardSteel AISI 1018
Yield strengthnot given (tensile used)producer-stated372MPa1
Ultimate tensile strength60MPa2producer-stated441MPa17.35x stronger
Flexural strength105MPa2not sourced
Elongation at break8%2in 2 in15%11.88x more ductile
Young's modulus (stiffness)2.75GPa2base material200GPa3
Density1,210kg/m³4base material7,861kg/m³3
Strength to weight49.6kN·m/kg5% higher47.3kN·m/kg
Stiffness to weight2.27MN·m/kg25.4MN·m/kg11.2x higher
Poisson's rationot sourcedbase material0.323
Shear modulusnot sourced75.7GPa
Bulk modulusnot sourced185GPa
Speed of sound1,508m/s5,043m/s3.34x faster
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumStainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30SLA Resin StandardSteel AISI 1018
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumStainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30SLA Resin StandardSteel AISI 1018
Strength against densityHigher and further left: stronger for its weight
ThermalSLA Resin StandardSteel AISI 1018
Thermal conductivity0.54W/m·K5base material51.9W/m·K3
Thermal expansionmean -30 to 140 °C114µm/m·K5base material12µm/m·K69.51x less
100 mm part over a 50 °C swing571µm growth60µm growth9.51x less
Specific heat1,800J/kg·K5base material486J/kg·K3
Heats up and cools (diffusivity)0.248mm²/s13.6mm²/s54.8x faster
Thermal shock resistancenot sourced5,473W/m
Max service temperatureHDT 1.8 MPa59°C2not sourced
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumStainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30SLA Resin StandardSteel AISI 1018
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumStainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30SLA Resin StandardSteel AISI 1018
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources6 documents: Niagara LaSalle, Formlabs, U.S. Department of Defense, Ovako
SLA Resin Standard
Formlabs Clear Resin V5 (FLGPCL05), TDS Rev. 01 March 20, 2024; printed on Form 4 at 100 µm, washed 5 min in >=99% IPA, post-cured 15 min at 60 °C in Form Cure. Orientation not stated.
Steel AISI 1018
AISI 1018 cold drawn bar (Niagara LaSalle, cold-finished bar producer)
  1. 1
    1018 PropertiesNiagara LaSallearchived copySteel AISI 1018 · Yield strength: producer-stated, cold drawnSteel AISI 1018 · Ultimate tensile strength: producer-stated, cold drawnSteel AISI 1018 · Elongation at break: in 2 in (50.8 mm)
  2. 2
    Clear Resin V5 Technical Data Sheet (2024)Formlabsarchived copySLA Resin Standard · Ultimate tensile strength: typicalSLA Resin Standard · Flexural strength: typicalSLA Resin Standard · Elongation at break: typicalSLA Resin Standard · Young's modulus (stiffness): typicalSLA Resin Standard · Max service temperature: HDT 1.8 MPa
  3. 3
    MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseSteel AISI 1018 · Young's modulus (stiffness): base material: AISI 1025 plain carbon steel (MIL-HDBK-5J design value; ASTM A108 bar is the cold-finished carbon-steel bar spec that also covers 1018)Steel AISI 1018 · Density: base material: AISI 1025 plain carbon steel (MIL-HDBK-5J design value; ASTM A108 bar is the cold-finished carbon-steel bar spec that also covers 1018)Steel AISI 1018 · Poisson's ratio: base material: AISI 1025 plain carbon steel (MIL-HDBK-5J design value; ASTM A108 bar is the cold-finished carbon-steel bar spec that also covers 1018)Steel AISI 1018 · Thermal conductivity: base material: AISI 1025 plain carbon steel (MIL-HDBK-5J design value; ASTM A108 bar is the cold-finished carbon-steel bar spec that also covers 1018)Steel AISI 1018 · Specific heat: base material: AISI 1025 plain carbon steel (MIL-HDBK-5J design value; ASTM A108 bar is the cold-finished carbon-steel bar spec that also covers 1018)
  4. 4
    Clear Resin V5 Technical Data Sheet (web edition)FormlabsSLA Resin Standard · Density: typical, post-cured (same for 5 min ambient and 15 min at 60 °C), ASTM D792
  5. 5
    Thermal Properties of Selected Formlabs SLA ResinsFormlabsSLA Resin Standard · Thermal conductivity: typical, post-cured, ASTM E1530SLA Resin Standard · Thermal expansion: mean -30 to 140 °C, post-cured (5 min ambient cure), TMA ASTM E831SLA Resin Standard · Specific heat: typical, 25 °C, post-cured (5 min ambient cure), DSC ASTM E1269
  6. 6
    S275JR Steel GradeOvakoSteel AISI 1018 · Thermal expansion: base material: unalloyed carbon steel, Ovako family table (S275JR, 'none alloyed structural steels', C <= 0.21%); mean 20-300 °C

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

SLA Resin Standard is 3D printed: its properties depend on build direction and print settings; these are typical values.

Questions

Mechanical

Is SLA Resin Standard stronger than Steel AISI 1018?

Steel AISI 1018 is stronger: its yield strength is 372 MPa against tensile strength 60 MPa for SLA Resin Standard (6.2x).

Which is lighter, SLA Resin Standard or Steel AISI 1018?

SLA Resin Standard is lighter: 1,210 kg/m³ against 7,861 kg/m³ for Steel AISI 1018.

Which is stiffer, SLA Resin Standard or Steel AISI 1018?

Steel AISI 1018 is stiffer: Young's modulus 200 GPa against 2.75 GPa for SLA Resin Standard, so the same part in Steel AISI 1018 deflects less under the same load.

Which is lighter for the same job, SLA Resin Standard or Steel AISI 1018?

For the same stiffness or strength: SLA Resin Standard is lighter for a stiff panel or plate, strong rod or tie, strong beam, strong panel or plate; Steel AISI 1018 is lighter for a stiff rod or tie (tension), stiff beam (bending).

Part that must beSLA Resin StandardSteel AISI 1018
Stiff rod or tie (tension)11.2x heavierlighter
Stiff beam (bending)31% heavierlighter
Stiff panel or platelighter1.56x heavier
Strong rod or tielighter5% heavier
Strong beamlighter1.93x heavier
Strong panel or platelighter2.61x heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, SLA Resin Standard or Steel AISI 1018?

Steel AISI 1018 stretches further before it breaks: 15% elongation at break against 8% for SLA Resin Standard.

Thermal

Which conducts heat better, SLA Resin Standard or Steel AISI 1018?

Steel AISI 1018 conducts heat better: 51.9 W/m·K against 0.54 W/m·K for SLA Resin Standard.

Which expands less with temperature?

Steel AISI 1018 expands less: 12 µm/m·K against 114 µm/m·K for SLA Resin Standard.