Materials / Compare

SLA Resin Standard vs. Steel AISI 4340

Compare SLA Resin Standard vs. Steel AISI 4340 strength, stiffness, weight and thermal properties.

SLA Resin Standard3D printed (SLA resin)
Steel AISI 4340Wrought
MechanicalSLA Resin StandardSteel AISI 4340
Yield strengthnot given (tensile used)1,035MPa1
Ultimate tensile strength60MPa21,140MPa119x stronger
Flexural strength105MPa2not sourced
Elongation at break8%218%12.25x more ductile
Young's modulus (stiffness)2.75GPa2200GPa3
Density1,210kg/m³46.48x lighter7,840kg/m³1
Strength to weight49.6kN·m/kg132kN·m/kg2.66x higher
Stiffness to weight2.27MN·m/kg25.5MN·m/kg11.2x higher
Poisson's rationot sourced0.323
Shear modulusnot sourced75.7GPa
Bulk modulusnot sourced185GPa
Speed of sound1,508m/s5,049m/s3.35x faster
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30SLA Resin StandardSteel AISI 4340
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30SLA Resin StandardSteel AISI 4340
Strength against densityHigher and further left: stronger for its weight
ThermalSLA Resin StandardSteel AISI 4340
Thermal conductivity0.54W/m·K537.5W/m·K169.4x more heat through a fin
Thermal expansionmean -30 to 140 °C114µm/m·K5mean11.3µm/m·K110.1x less
100 mm part over a 50 °C swing571µm growth56.5µm growth10.1x less
Specific heat1,800J/kg·K54.02x higher448J/kg·K1
Heats up and cools (diffusivity)0.248mm²/s10.7mm²/s43x faster
Thermal shock resistancenot sourced11,678W/m
Max service temperatureHDT 1.8 MPa59°C2not sourced
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30SLA Resin StandardSteel AISI 4340
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30SLA Resin StandardSteel AISI 4340
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources5 documents: Carpenter Technology, Formlabs, U.S. Department of Defense
SLA Resin Standard
Formlabs Clear Resin V5 (FLGPCL05), TDS Rev. 01 March 20, 2024; printed on Form 4 at 100 µm, washed 5 min in >=99% IPA, post-cured 15 min at 60 °C in Form Cure. Orientation not stated.
Steel AISI 4340
Carpenter (Latrobe) Lescalloy 4340 VAC-ARC datasheet; mechanical row for 1100 °F temper; physical properties grade-level
  1. 1
    Lescalloy 4340 VAC-ARC Data SheetCarpenter Technologyarchived copySteel AISI 4340 · Yield strength: typical, transverseSteel AISI 4340 · Ultimate tensile strength: typical, transverseSteel AISI 4340 · Elongation at break: typical, transverseSteel AISI 4340 · Density: typicalSteel AISI 4340 · Thermal conductivity: typicalSteel AISI 4340 · Thermal expansion: mean, -18 to 93 °CSteel AISI 4340 · Specific heat: typical
  2. 2
    Clear Resin V5 Technical Data Sheet (2024)Formlabsarchived copySLA Resin Standard · Ultimate tensile strength: typicalSLA Resin Standard · Flexural strength: typicalSLA Resin Standard · Elongation at break: typicalSLA Resin Standard · Young's modulus (stiffness): typicalSLA Resin Standard · Max service temperature: HDT 1.8 MPa
  3. 3
    MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseSteel AISI 4340 · Young's modulus (stiffness): MIL-HDBK-5J design value (AISI 4340, quenched and tempered)Steel AISI 4340 · Poisson's ratio: MIL-HDBK-5J design value (AISI 4340, quenched and tempered)
  4. 4
    Clear Resin V5 Technical Data Sheet (web edition)FormlabsSLA Resin Standard · Density: typical, post-cured (same for 5 min ambient and 15 min at 60 °C), ASTM D792
  5. 5
    Thermal Properties of Selected Formlabs SLA ResinsFormlabsSLA Resin Standard · Thermal conductivity: typical, post-cured, ASTM E1530SLA Resin Standard · Thermal expansion: mean -30 to 140 °C, post-cured (5 min ambient cure), TMA ASTM E831SLA Resin Standard · Specific heat: typical, 25 °C, post-cured (5 min ambient cure), DSC ASTM E1269

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

SLA Resin Standard is 3D printed: its properties depend on build direction and print settings; these are typical values.

Questions

Mechanical

Is SLA Resin Standard stronger than Steel AISI 4340?

Steel AISI 4340 is stronger: its yield strength is 1,035 MPa against tensile strength 60 MPa for SLA Resin Standard (17.3x).

Which is lighter, SLA Resin Standard or Steel AISI 4340?

SLA Resin Standard is lighter: 1,210 kg/m³ against 7,840 kg/m³ for Steel AISI 4340.

Which is stiffer, SLA Resin Standard or Steel AISI 4340?

Steel AISI 4340 is stiffer: Young's modulus 200 GPa against 2.75 GPa for SLA Resin Standard, so the same part in Steel AISI 4340 deflects less under the same load.

Which is lighter for the same job, SLA Resin Standard or Steel AISI 4340?

For the same stiffness or strength: SLA Resin Standard is lighter for a stiff panel or plate, strong panel or plate; Steel AISI 4340 is lighter for a stiff rod or tie (tension), stiff beam (bending), strong rod or tie, strong beam.

Part that must beSLA Resin StandardSteel AISI 4340
Stiff rod or tie (tension)11.2x heavierlighter
Stiff beam (bending)32% heavierlighter
Stiff panel or platelighter1.55x heavier
Strong rod or tie2.66x heavierlighter
Strong beam3% heavierlighter
Strong panel or platelighter1.56x heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, SLA Resin Standard or Steel AISI 4340?

Steel AISI 4340 stretches further before it breaks: 18% elongation at break against 8% for SLA Resin Standard.

Thermal

Which conducts heat better, SLA Resin Standard or Steel AISI 4340?

Steel AISI 4340 conducts heat better: 37.5 W/m·K against 0.54 W/m·K for SLA Resin Standard.

Which expands less with temperature?

Steel AISI 4340 expands less: 11.3 µm/m·K against 114 µm/m·K for SLA Resin Standard.