Materials / Compare

Steel vs. Wood

Compare Steel vs. Wood strength, stiffness, weight and thermal properties.

SteelWrought
WoodNatural
MechanicalSteelWood
Yield strength385MPa1not given (tensile used)
Ultimate tensile strength505MPa1modulus of rupture99MPa2
Compressive strengthnot sourced46.6MPa2
Flexural strengthnot sourcedmodulus of rupture99MPa2
Elongation at break24.2%1not sourced
Young's modulus (stiffness)design value200GPa3bending MOE12.5GPa2
Density7,850kg/m³4681–702kg/m³5
Strength to weight49kN·m/kg143kN·m/kg2.92x higher
Stiffness to weight25.5MN·m/kg41% higher18.1MN·m/kg
Poisson's ratiodesign value0.33mu_LR0.352
Shear modulus76.9GPa16.6x stiffer in shear4.63GPa
Bulk modulus167GPa12x higher13.9GPa
Speed of sound5,048m/s19% faster4,252m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonAluminumIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30SteelWood
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberAluminumIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30SteelWood
Strength against densityHigher and further left: stronger for its weight
ThermalSteelWood
Thermal conductivity48W/m·K4267x more heat through a finacross grain0.18W/m·K6
Thermal expansion12µm/m·K4parallel to grain3.1–4.5µm/m·K6
100 mm part over a 50 °C swing60µm growth19µm growth3.16x less
Specific heatbase material460–480J/kg·K7solid wood1,700J/kg·K6
Heats up and cools (diffusivity)13mm²/s85x faster0.153mm²/s
Thermal shock resistance5,390W/m22.1x more resistant244W/m
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberAluminumIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30SteelWood
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonAluminumIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30SteelWood
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources7 documents: American Institute of Steel Construction, USDA Forest Products Laboratory, bauforumstahl (ArcelorMittal), Ovako
Steel
Generic structural steel, cited as ASTM A992 (the current US structural grade): ASTM A992 W-shapes; Fy/Fu specified minimums from AISC publications (AISC 360-16 Commentary; Modern Steel Construction); elastic constants AISC 360; physical constants from the bauforumstahl structural-steel EPD, which names A992 among covered product standards.
Wood
Northern red oak (Quercus rubra), clear straight-grained specimens at 12% MC, parallel to grain unless stated; USDA FPL Wood Handbook FPL-GTR-282 (2021) Ch. 4 and Ch. 5
  1. 1
    Updating Standard Shape Material Properties Database for Design and ReliabilityAmerican Institute of Steel Constructionarchived copySteel · Yield strength: typical: mean of 20,295 A992 flange mill-test coupons (1998 SSPC survey), as reported by AISCSteel · Ultimate tensile strength: typical: mean of 20,295 A992 flange mill-test coupons (1998 SSPC survey)Steel · Elongation at break: typical: mean of 24,847 A992 mill-test elongations, web and flange (1998 SSPC mill data), as reported by AISC
  2. 2
    Wood Handbook (FPL-GTR-282), Chapter 5: Mechanical Properties of WoodUSDA Forest Products LaboratoryWood · Ultimate tensile strength: modulus of rupture (no direct tensile value)Wood · Compressive strength: compression parallel to grain (maximum crushing strength), 12% MCWood · Flexural strength: modulus of rupture (static bending), 12% MCWood · Young's modulus (stiffness): bending MOE, parallel to grainWood · Poisson's ratio: mu_LR (red oak group, ~12% MC)
  3. 3
    ANSI/AISC 360-16 Specification for Structural Steel Buildings, with CommentaryAmerican Institute of Steel Constructionarchived copySteel · Young's modulus (stiffness): design value (AISC 360-16)Steel · Poisson's ratio: design value (AISC 360-16 Commentary)
  4. 4
    Environmental Product Declaration: Structural Steel Sections and Merchant Bars (2023)bauforumstahl (ArcelorMittal)archived copySteel · Density: nominal (constructional data)Steel · Thermal conductivity: nominal at 20 °CSteel · Thermal expansion: nominal (constructional data, no temperature range stated)
  5. 5
    Technical Note 218: Weights of Various Woods Grown in the United States (1953)USDA Forest Products LaboratoryWood · Density: average weight of clear wood at 8% and 15% moisture content
  6. 6
    Wood Handbook (FPL-GTR-282), Chapter 4: Moisture Relations and Physical Properties of WoodUSDA Forest Products LaboratoryWood · Thermal conductivity: across grain, 12% MC (Table 4-7, approximate)Wood · Thermal expansion: parallel to grain, ovendry wood, range across speciesWood · Specific heat: solid wood (all species), 12% MC, 27 C
  7. 7
    S275JR Steel GradeOvakoSteel · Specific heat: base material: EN S275JR unalloyed structural steel (the EN counterpart of A36), typical, 50/100 °C

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Questions

Mechanical

Is Steel stronger than Wood?

Steel is stronger: its yield strength is 385 MPa against tensile strength 99 MPa for Wood (3.89x).

Which is lighter, Steel or Wood?

Wood is lighter: 692 kg/m³ against 7,850 kg/m³ for Steel.

Which is stiffer, Steel or Wood?

Steel is stiffer: Young's modulus 200 GPa against 12.5 GPa for Wood, so the same part in Steel deflects less under the same load.

Which is lighter for the same job, Steel or Wood?

For the same stiffness or strength: Steel is lighter for a stiff rod or tie (tension); Wood is lighter for a stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.

Part that must beSteelWood
Stiff rod or tie (tension)lighter41% heavier
Stiff beam (bending)2.84x heavierlighter
Stiff panel or plate4.51x heavierlighter
Strong rod or tie2.92x heavierlighter
Strong beam4.59x heavierlighter
Strong panel or plate5.76x heavierlighter

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Thermal

Which conducts heat better, Steel or Wood?

Steel conducts heat better: 48 W/m·K against 0.18 W/m·K for Wood.

Which expands less with temperature?

Wood expands less: 3.8 µm/m·K against 12 µm/m·K for Steel.

Related comparisons