Mechanical
Yield strength69MPa1
Ultimate tensile strength221MPa1
Elongation at break45%1
Young's modulus (stiffness)117GPa1
Density8,941kg/m³1
Strength to weight7.72kN·m/kg
Stiffness to weight13.1MN·m/kg
Poisson's ratio0.342
Shear modulus43.7GPa
Bulk modulus122GPa
Speed of sound3,621m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Copper C10100
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Copper C10100
Strength against densityHigher and further left: stronger for its weight
Thermal
Thermal conductivity391W/m·K1
Thermal expansion16.9µm/m·K1
100 mm part over a 50 °C swing84.5µm growth
Specific heat385J/kg·K1
Heats up and cools (diffusivity)114mm²/s
Thermal shock resistance8,992W/m
Melting pointmelting point1,083°C1
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Copper C10100
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Copper C10100
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Sources2 documents: Copper Development Association, Wieland
Values for
Wrought. C10100 oxygen-free electronic (OFE) copper, annealed to 0.050 mm grain size (OS050), 0.04 in. flat products, copper.org typical values
  1. 1
    C10100 Alloy (copper.org)Copper Development Associationarchived copyYield strength: typical, 0.5% extension under load, 0.04 in. flatUltimate tensile strength: typical, 0.04 in. flatElongation at break: typical, 0.04 in. flatYoung's modulus (stiffness): typicalDensity: nominalThermal conductivity: typical, 20 °CThermal expansion: typical, mean 20-100 °CSpecific heat: typical, 20 °CMelting point: melting point (liquidus = solidus, pure copper)
  2. 2
    Wieland-K09 (Cu-OFE, C10100) Data SheetWielandPoisson's ratio: reference value at room temperature (Wieland-K09 = Cu-OFE = C10100, rolled products)

Thermal properties of Copper C10100

Thermal conductivity of Copper C10100

Copper C10100 has a thermal conductivity of 391 W/m·K (226 BTU/hr·ft·°F). Basis: typical, 20 °C. Source: Copper Development Association, C10100 Alloy (copper.org)archived copy.

Specific heat of Copper C10100

The specific heat capacity of Copper C10100 is 385 J/kg·K (0.092 BTU/lb·°F). Basis: typical, 20 °C. Source: Copper Development Association, C10100 Alloy (copper.org)archived copy.

Coefficient of thermal expansion of Copper C10100

Copper C10100 expands 16.9 µm/m·K (9.39 µin/in·°F): a 100 mm part grows 84.5 µm over a 50 °C rise. Basis: typical, mean 20-100 °C. Source: Copper Development Association, C10100 Alloy (copper.org)archived copy.

Thermal diffusivity of Copper C10100

Computed from the conductivity, density and specific heat (k / ρc): 114 mm²/s, how fast a temperature change spreads through it.

Melting point of Copper C10100

Copper C10100 melts at 1,083 °C (1,981 °F). Basis: melting point (liquidus = solidus, pure copper). Source: Copper Development Association, C10100 Alloy (copper.org)archived copy.