Materials / SLS

SLS PA12 Nylon

SLS PA12 Nylon strength, stiffness, density and thermal properties, with their source.

A bracket in SLS PA12 Nylon, as-sintered finish.

Process3D printed (SLS)
Mechanical
Yield strengthnot given (tensile used)
Ultimate tensile strength48MPasourcetypical
Elongation at break18%sourcetypical
Young's modulus (stiffness)1.65GPasourcetypical
Density930kg/m³sourcetypical
Strength to weight51.6kN·m/kg
Stiffness to weight1.77MN·m/kg
Poisson's rationot sourced
Shear modulusnot sourced
Bulk modulusnot sourced
Speed of sound1,332m/s
Thermal
Thermal conductivitynot sourced
Thermal expansionnot sourced
100 mm part over a 50 °C swingnot sourced
Specific heatnot sourced
Heats up and cools (diffusivity)not sourced
Thermal shock resistancenot sourced
Melting point176°Csourcetypical
Max service temperature64°CsourceHDT 1.8 MPa, X orientation
Values forEOS PA 2200 (PA12) Material Data Sheet, process parameter 'Balance' at 120 µm layer thickness, X orientation, dry (conditioned values not given). Live MDS status 04.10.2026, last changed 10.09.2026; PDF via ?topdf=... link on the same page.

SLS PA12 Nylon is 3D printed: its properties depend on build direction and print settings; these are typical values.

Among 59 materials

1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000DMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelSLS PA12 Nylon
Stiffness against density
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLA Resin Elastic 50ADMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickSLS PA12 Nylon
Strength against density

Compare SLS PA12 Nylon with