Materials / Steel

Steel AISI 1045

Steel AISI 1045 (medium carbon, cold drawn) strength, stiffness, density and thermal properties, with their source.

A bracket in Steel AISI 1045, brushed finish.

ProcessWrought
Mechanical
Yield strength531MPasourceproducer-stated, cold drawn
Ultimate tensile strength627MPasourceproducer-stated, cold drawn
Elongation at break12%sourcein 2 in (50.8 mm)
Young's modulus (stiffness)210GPasourcetypical
Density7,800kg/m³sourcetypical
Strength to weight68.1kN·m/kg
Stiffness to weight26.9MN·m/kg
Poisson's ratio0.3sourcetypical
Shear modulus80.8GPa
Bulk modulus175GPa
Speed of sound5,189m/s
Thermal
Thermal conductivity40–45W/m·Ksourcetypical range, ambient
Thermal expansion12µm/m·Ksourcetypical, mean 20-300 °C
100 mm part over a 50 °C swing60µm growth
Specific heat460–480J/kg·Ksourcetypical range, 50/100 °C
Heats up and cools (diffusivity)11.6mm²/s
Thermal shock resistance6,269W/m
Values forAISI 1045 cold drawn bar (Niagara LaSalle) for mechanical; Ovako C45 (lists 'SAE 1045' as a similar designation) for physical constants

Among 59 materials

1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelSteel AISI 1045
Stiffness against density
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickSteel AISI 1045
Strength against density

Compare Steel AISI 1045 with