ProcessWrought
Mechanical
Yield strength276MPasourcetypical, 0.2% offset, .500 in dia specimen
Ultimate tensile strength310MPasourcetypical
Elongation at break17%sourcetypical, in 4D, 0.500 in dia specimen
Young's modulus (stiffness)68.3GPasourcetypical
Density2,700kg/m³sourcenominal
Strength to weight102kN·m/kg
Stiffness to weight25.3MN·m/kg
Poisson's ratio0.33sourcetypical (handbook physical constant)
Shear modulus25.7GPa
Bulk modulus67GPa
Speed of sound5,030m/s
Thermal
Thermal conductivity167W/m·Ksourcetypical, 20 °C
Thermal expansion23.6µm/m·Ksourcetypical, mean 20-100 °C
100 mm part over a 50 °C swing118µm growth
Specific heat896J/kg·Ksourcetypical, at 100 °C
Heats up and cools (diffusivity)69mm²/s
Thermal shock resistance19,159W/m
Melting point582–652°Csourcesolidus-liquidus
Values for6061-T6/T651, Kaiser Aluminum typical properties; Poisson from MIL-HDBK-5J

Among 59 materials

1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelAluminum 6061-T6
Stiffness against density
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickAluminum 6061-T6
Strength against density

Compare Aluminum 6061-T6 with