Materials / Compare

Aluminum 5052-H32 vs. Plastic UHMWPE

Compare Aluminum 5052-H32 vs. Plastic UHMWPE strength, stiffness, weight and thermal properties.

Aluminum 5052-H32Wrought
Plastic UHMWPEBulk polymer (molded or machined)
MechanicalAluminum 5052-H32Plastic UHMWPE
Yield strength195MPa19.75x stronger20MPa2
Ultimate tensile strength230MPa143MPa2
Elongation at break12%1465%238.8x more ductile
Young's modulus (stiffness)70GPa1106x stiffer0.66GPa2
Density2,685kg/m³3930kg/m³22.89x lighter
Strength to weight72.6kN·m/kg3.38x higher21.5kN·m/kg
Stiffness to weight26.1MN·m/kg36.7x higher0.71MN·m/kg
Poisson's ratio0.333not sourced
Shear modulus26.3GPanot sourced
Bulk modulus68.6GPanot sourced
Speed of sound5,106m/s6.06x faster842m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 5052-H32Plastic UHMWPE
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 5052-H32Plastic UHMWPE
Strength against densityHigher and further left: stronger for its weight
ThermalAluminum 5052-H32Plastic UHMWPE
Thermal conductivitybase material138W/m·K1345x more heat through a fin0.4W/m·K4
Thermal expansion23.8µm/m·K18.4x less200µm/m·K4
100 mm part over a 50 °C swing119µm growth8.4x less1,000µm growth
Specific heatat 100 °C963J/kg·K3not sourced
Heats up and cools (diffusivity)53.4mm²/snot sourced
Thermal shock resistance10,822W/mnot sourced
Melting pointmelting range605–650°C1DSC 10 K/min130–138°C2
Max service temperaturenot sourced80°C2
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 5052-H32Plastic UHMWPE
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 5052-H32Plastic UHMWPE
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources4 documents: Kaiser Aluminum, Celanese, U.S. Department of Defense
Aluminum 5052-H32
5052-H32, Kaiser Aluminum tube & pipe typical datasheet (mechanical, CTE, melting); MIL-HDBK-5J (Poisson, density, specific heat)
Plastic UHMWPE
Celanese GUR 4120 (avg. molecular weight 4.7x10^6 g/mol), typical values on compression-molded specimens; CTE and thermal conductivity from Celanese's generic UHMWPE guide (grade not named)
  1. 1
    Alloy 5052 Tube & Pipe Technical DataKaiser Aluminumarchived copyAluminum 5052-H32 · Yield strength: typical, 0.2% offsetAluminum 5052-H32 · Ultimate tensile strength: typicalAluminum 5052-H32 · Elongation at break: typicalAluminum 5052-H32 · Young's modulus (stiffness): typicalAluminum 5052-H32 · Thermal conductivity: base material: 5052 in O temper (same alloy, annealed); Kaiser typicalAluminum 5052-H32 · Thermal expansion: typical, mean 20-100 °CAluminum 5052-H32 · Melting point: melting range
  2. 2
    GUR UHMW-PE Overview (GUR-015)CelanesePlastic UHMWPE · Yield strength: typical, tensile stress at yield ISO 527, 50 mm/minPlastic UHMWPE · Ultimate tensile strength: typical, tensile stress at break ISO 527, 50 mm/minPlastic UHMWPE · Elongation at break: typical, nominal elongation at break ISO 527Plastic UHMWPE · Young's modulus (stiffness): typical, tensile modulus ISO 527, 1 mm/minPlastic UHMWPE · Density: typicalPlastic UHMWPE · Melting point: DSC 10 K/minPlastic UHMWPE · Max service temperature: recommended max constant operating temperature
  3. 3
    MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseAluminum 5052-H32 · Density: nominalAluminum 5052-H32 · Poisson's ratio: typical (handbook physical constant)Aluminum 5052-H32 · Specific heat: at 100 °C (212 °F); table covers O, H32, H34, H36, H38
  4. 4
    GUR UHMW-PE Polymer Guide (GUR-003)Celanesearchived copyPlastic UHMWPE · Thermal conductivity: typical, unfilled (narrative value, generic Celanese UHMWPE)Plastic UHMWPE · Thermal expansion: typical, 20 to 100 °C (generic Celanese UHMWPE)

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Questions

Mechanical

Is Aluminum 5052-H32 stronger than Plastic UHMWPE?

Aluminum 5052-H32 is stronger: its yield strength is 195 MPa against 20 MPa for Plastic UHMWPE (9.75x).

Which is lighter, Aluminum 5052-H32 or Plastic UHMWPE?

Plastic UHMWPE is lighter: 930 kg/m³ against 2,685 kg/m³ for Aluminum 5052-H32.

Which is stiffer, Aluminum 5052-H32 or Plastic UHMWPE?

Aluminum 5052-H32 is stiffer: Young's modulus 70 GPa against 0.66 GPa for Plastic UHMWPE, so the same part in Aluminum 5052-H32 deflects less under the same load.

Which is lighter for the same job, Aluminum 5052-H32 or Plastic UHMWPE?

For the same stiffness or strength: Aluminum 5052-H32 is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.

Part that must beAluminum 5052-H32Plastic UHMWPE
Stiff rod or tie (tension)lighter36.7x heavier
Stiff beam (bending)lighter3.57x heavier
Stiff panel or platelighter1.64x heavier
Strong rod or tielighter3.38x heavier
Strong beamlighter1.58x heavier
Strong panel or platelighter8% heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Aluminum 5052-H32 or Plastic UHMWPE?

Plastic UHMWPE stretches further before it breaks: 465% elongation at break against 12% for Aluminum 5052-H32.

Thermal

Which conducts heat better, Aluminum 5052-H32 or Plastic UHMWPE?

Aluminum 5052-H32 conducts heat better: 138 W/m·K against 0.4 W/m·K for Plastic UHMWPE.

Which expands less with temperature?

Aluminum 5052-H32 expands less: 23.8 µm/m·K against 200 µm/m·K for Plastic UHMWPE.

Related comparisons