Materials / Plastic

Plastic UHMWPE

Plastic UHMWPE strength, stiffness, density and thermal properties, with their source.

A bracket in Plastic UHMWPE, smooth finish.

ProcessBulk polymer (molded or machined)
Mechanical
Yield strength20MPasourcetypical, tensile stress at yield ISO 527, 50 mm/min
Ultimate tensile strength43MPasourcetypical, tensile stress at break ISO 527, 50 mm/min
Elongation at break465%sourcetypical, nominal elongation at break ISO 527
Young's modulus (stiffness)0.66GPasourcetypical, tensile modulus ISO 527, 1 mm/min
Density930kg/m³sourcetypical
Strength to weight21.5kN·m/kg
Stiffness to weight0.71MN·m/kg
Poisson's rationot sourced
Shear modulusnot sourced
Bulk modulusnot sourced
Speed of sound842m/s
Thermal
Thermal conductivity0.4W/m·Ksourcetypical, unfilled (narrative value, generic Celanese UHMWPE)
Thermal expansion200µm/m·Ksourcetypical, 20 to 100 °C (generic Celanese UHMWPE)
100 mm part over a 50 °C swing1,000µm growth
Specific heatnot sourced
Heats up and cools (diffusivity)not sourced
Thermal shock resistancenot sourced
Melting point130–138°CsourceDSC 10 K/min
Max service temperature80°Csourcerecommended max constant operating temperature
Values forCelanese GUR 4120 (avg. molecular weight 4.7x10^6 g/mol), typical values on compression-molded specimens; CTE and thermal conductivity from Celanese's generic UHMWPE guide (grade not named)

Among 59 materials

1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelPlastic UHMWPE
Stiffness against density
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPlastic UHMWPE
Strength against density

Compare Plastic UHMWPE with